Saturday, November 23, 2024, 11:11, Darwin Ortiz Rosales, ZrC, , LP TUBE, Done, ZrC 24E9T1 + std conditioning and sintering
|
Saturday, November 23, 2024, 11:08
No milling ZrC material sintering inside graphite cartridge
baseline standard discs included for comparison.
4 Ta foils wrapped around container
one spring at the back end to retain the graphite cartridge
One Ta cap with perforations at the front for T readings
initial heating at 2A/min to 50A, followed by heating at 1A/min to 90 A
Initial IGP1= 1.0e-6 Torr
OMEGA slope =0.990
Good and bad vacuum =5.0e-5 Torr and 5e-4 torr
Saturday, November 23, 2024, 11:20
autoramp start at 2A/min to 50A on tght
Saturday, November 23, 2024, 20:11
allowed pressure to drop to 3.3e-6 Torr after degassing.
Started ramp to 90A at 1A/min
Saturday, November 23, 2024, 23:46
started ramping at 1.5A/120s or 0.75A/min to 400A
Sunday, November 24, 2024, 07:55
Reached 1900 C at 410 A setpoint and 402 A on RD
Pressure did not increase after bumping up to 410 setpoint so will keep at this current until 11 am (four hours near 1900 C in total)
Sunday, November 24, 2024, 10:58
Final IGP1 at start of rampdown = 2.9e-6 Torr
Ramping down at -2A/min |
Wednesday, October 02, 2024, 19:24, Darwin Ortiz Rosales, TiC, , LP TUBE, Done, sintering TiC Experiment
|
Wednesday, October 02, 2024, 19:21
Ta endcup at front end of container
End-caps on the graphite cartridge have holes for outgassing.
initial heating @ 2A/min to 85 A then 2A/min to 120A TGHT. Allow pressure to drop and then ramp to 400 A at 2A/min, leave 4 hours and start ramp down.
OMEGA slope = 0.99
Vacuum limits up to 400A: 5.0e-04 Torr -- 1.0e-02 Torr
Max current~400A (1900 C)
Wednesday, October 02, 2024, 19:25
Starting IGP1 = 6.65e-06 Torr
Thursday, October 03, 2024, 05:09
Starting rampdown. Pressure stable at 4.5 e-06 Torr
Top temperature 1850 C on OMEGA
ramping down at -2A/min |
Tuesday, September 10, 2024, 13:16, Darwin Ortiz Rosales, Endcaps, , TARGET BOAT, Done, TaC coating sintering
|
A boat lined up with graphite and wrapped in 3 Ta heatshileds
Vacuum IGP1 initial =6.1 e-06 Torr
Target temperature on OMEGA= 1800-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final TGHT current= ~400A (adjustable)
Heating autoramp started semi-manually on TGHT to 65A and then at continue to 100A
After peak heat at 1A/min to =400 A TGHT
Good vacuum = 5.0 e-04 Torr
Bad vacuum = 5.0E-02 Torr
Tuesday, September 10, 2024, 22:22
1810C OMEGA at 439A TGHT readback |
Monday, September 09, 2024, 19:08, Darwin Ortiz Rosales, TaC, , LP-SIS, Done, TaC coating sintering LP-SIS with gas line
|
Monday, September 09, 2024, 19:06
The coated container was wrapped in 4 Ta foil heatshields.
Vacuum IGP1 initial =2.6 e-06 Torr
Target temperature on OMEGA= 1800-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230 A
Final TGHT current= ~400A (adjustable)
Heating autoramp starged at 1A/min on TGHT and TBHT until outgassin peak passed
Then at 1A/min to =400 A TGHT and 230A TBHT
Good vacuum = 5.0 e-04 Torr
Bad vacuum = 5.0E-02 Torr
Monday, September 09, 2024, 19:08
Peak passed around 70A will continue ramp up at 1A/min to 400A on TGHT and 230A TBHT
Tuesday, September 10, 2024, 13:13
Was ramped down at -2 A/min TGHT and -1 A/min TBHT
|
Saturday, September 07, 2024, 09:55, Darwin Ortiz Rosales, TaC, 45447-13, LP-SIS, Done, TaC coating sintering
|
Saturday, September 07, 2024, 09:54
The coated container was wrapped in 4 Ta foil heatshields.
Vacuum IGP1 initial =8.1 e-07 Torr
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230 A
Final TGHT current= ~400A (adjustable)
Heating ramp manually to 50A on TGHT and TBHT
Then at 1A/min to =400 A TGHT and 230A TBHT
Good vacuum = 5.0 e-04 Torr
Bad vacuum = 5.0E-02 Torr
Saturday, September 07, 2024, 17:38
At 400 A set point on TGHT, read back is 392A and OMEGA reads 1840C. TBHT set to 230A reads 233A.
It will be kept at this current for four hours before rampdown. |
Friday, August 30, 2024, 11:33, Darwin Ortiz Rosales, Ta, 45447-8, LP-IG-LIS, Done, TaC coating sintering
|
Friday, August 30, 2024, 11:31
The coated container was wrapped in 4 Ta foil heatshields.
Vacuum IGP1 initial =3.1 e-07 Torr
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230 A
Final TGHT current= ~400A (adjustable)
Heating autoramp starged at 1A/min on TGHT 100A and TBHT
Then at 1A/min to =400 A TGHT and 230A TBHT
Good vacuum = 5.0 e-04 Torr
Bad vacuum = 5.0E-02 Torr
note: Left TBHT hole is off from center by a good margin
Sunday, September 01, 2024, 07:32
Starting initial ramp at 1A/min to 50A
Sunday, September 01, 2024, 15:20
have ramped ;up at 1A/min on both TGHT and TBHT but had two issues.
1) Set current and readback current have discrepancies but the TBHT discrepancy is significant (TBHT Set at 188 while RD is 231.9 A @ 1.9V)
TGHT also has odd behavior with set point 405 giving 392A RD and 0.067V. Will hold until 430pm before starting ramp down
Sunday, September 01, 2024, 16:30
Started rampdown at -2A/min TGHT and -1A/min TBHT
Note: OMEGA not able to give any reasonable readings
Tuesday, September 03, 2024, 13:51
After troubleshooting EVAP2 it was found that a copper line was touching the metal encasement grid most likely resulting in a short. A short was seeing and it disappeared after moving the copper line away from the grid.
Upon restarting on epics the PS went to maximum current and it was shut off after 30seconds to a minute. The system was checked again by Arthur and TGHT was manually increased to 5A and then set to Zero again. Arthur thinks that the PS probably requires this step after switching from local controls to remote. Will start the sintering again as the container is coated but not sintered.
Tuesday, September 03, 2024, 14:03
ramping at 1A/min on both TGHT and TBHT to 90A.
Tuesday, September 03, 2024, 22:25
Started rampdown at -2A/min TGHT and -1A/min TBHT. HIgh temperature from OMEGA was 1825 C at 430A readback on TGHT. |
Monday, August 19, 2024, 13:17, John Wong, np-Ta, , TARGET BOAT, In progress, Carbonization of heat stabilized np-Ta fibres - 2nd Attempt
|
Monday, August 19, 2024, 13:06
Target container consists of 2 samples, and both samples were heat stabilized at 150 C for 24 hours then pre-oxidized at 360 C for 4 hours:
1. PVP (7% wt/v) spun fibres 0.0569 g
2. np-Ta (Dope 7) spun fibres: 0.1730 g
Samples are wrapped in graphite foil and loaded into a target boat which is wrapped with Ta foil.
Omega slope set at 0.99.
Similar heat treatment as the 1st attempt, see e-log #667 (1800 C = 402A/7.2V).
Good vac = 3 e-5 Torr
Bad vac = 5 e-5 Torr.
Chamber is currently pumping down.
Monday, August 19, 2024, 16:52
Chamber pressure @ 4.6e-6 Torr.
Initiate auto-ramping at 1A/min to reach 400A.
Continue to monitor the pressure and TGHT.
Tuesday, August 20, 2024, 09:48
TGHT reached 400 A/6.87V about 10 hr ago. But the temperature has been holding at 1665 C.
The voltage is much lower this time compared to the previous heat treatment. See attachment #1 for the overall process.
Ramping up to 450A. Continue monitoring..
Tuesday, August 20, 2024, 15:43
TGHT at 450A (readback 441A)/7.892V, temperature holding at 1803C
Pressure coming down from 1.62e-6 Torr.
Continue to hold on the temperature for a few more hours before cooling it down
Wednesday, August 21, 2024, 09:40
Temperature was holding for about 18 hours before ramping down TGHT was initiated at 2A/min.
The samples can be taken out after 2 pm.
|
Wednesday, August 14, 2024, 07:23, Marla Cervantes, C, 44139-5 SK, LP TUBE, Problems, EVAP2 Calibration - Vanadium
|
Tuesday, August 13, 2024, 17:20 Pressure kept increasing when turning the turbo pump on
Tuesday, August 13, 2024, 18:00 Pressure stayed constant when turning the turbo pump on |
Wednesday, August 14, 2024, 16:22, Marla Cervantes, C, 44139-5 SK, LP TUBE, Problems resolved, EVAP2 Calibration - Vanadium
|
Marla Cervantes wrote: |
Tuesday, August 13, 2024, 17:20 Pressure kept increasing when turning the turbo pump on
Tuesday, August 13, 2024, 18:00 Pressure stayed constant when turning the turbo pump on
|
Wednesday, August 14, 2024, 10:18
The turbo pump started up normally. System is purging. and tomorrow the target will be heated.
|
Wednesday, August 14, 2024, 16:24, Marla Cervantes, C, 44139-5 SK, LP TUBE, In progress, EVAP2 Calibration - Vanadium
|
Marla Cervantes wrote: |
Marla Cervantes wrote: |
Tuesday, August 13, 2024, 17:20 Pressure kept increasing when turning the turbo pump on
Tuesday, August 13, 2024, 18:00 Pressure stayed constant when turning the turbo pump on
|
Wednesday, August 14, 2024, 10:18
The turbo pump started up normally. System is purging. and tomorrow the target will be heated.
|
Wednesday, August 14, 2024, 16:19
A vanadium wire was introduced in a tantalum pouch and snug among the graphite foils of a conditioned graphite target. The V wire was introduced in the Ta pouch to prevent the direct contact of the wire with the carbon and avoid the reaction between them.
As a first approach, the target will be heated to approximately 1377 °C, aiming at the vaporization temperature of the V wire. If the wire does not vaporize, heating with the turbo pump off would be considered to aim at the vanadium's melting point of 1910 °C.
|
|
Vaporization (at 3e-6 Torr)
|
|
|
|
In case of outgassing, let the pressure reduce
- Next ramping: 0.5 A/ 2min to 250 A.
Very slow rate to allow thermal equilibrium and temperature measurements. Estimated time 3h.
Thursday, August 15, 2024, 08:21
IGP1 = 5.3e-7 Torr
Good vacuum 3e-5 Torr
Bad vacuum 5e-5 Torr
Initial ramping: 2 A/min to 200 A.
Thursday, August 15, 2024, 09:01. Pressure starting to increase at 74 A
Thursday, August 15, 2024, 09:15. Pressure stabilizing 1.8e-6 Torr. Current 103 A, voltage 1.3 V
Thursday, August 15, 2024, 09:21. Pressure increasing (116 A).
Thursday, August 15, 2024, 09:29 Pressure dropping (Current approx. 120 A)
Thursday, August 15, 2024, 10:54
Started ramping to find a pressure peak corresponding to V vaporization.
IGP1 = 6.4e-7
TGHT = 200 A, 2.9 V, omega 1152 °C
Next ramping: 0.5 A/ 2min to 250 A
Thursday, August 15, 2024, 11:17
Ramp seem to slow. The temperature change was too subtle (according to the omega).
IGP1 = 6.5e-7
TGHT = 205 A, 3.03 V, omega 1157 °C
Next ramping: 1 A/ 2min to 250 A
Thursday, August 15, 2024, 11:32
Ramp changed to 0.5 A/min
Thursday, August 15, 2024, 11:54
Ramp was stopped because the pressure was increasing, suggesting the V vaporization.
IGP1 = 6.9e-7
TGHT = 222 A, 3.3 V
Omega 1210 °C, filament 1280 °C
The difference between pyrometers is negligible, suggesting that the V vaporization temperature at 6e-7 Torr of approx. 1300 °C
Thursday, August 15, 2024, 13:15
IGP1 = 7.9e-7
TGHT = 250 A, 3.8 V
Omega 1289 °C
Thursday, August 15, 2024, 13:16
Ramp set to 0.5 A/min to 300 A
Pressure mini-spike at 13:18
Omega reading 1291 °C
Thursday, August 15, 2024, 14:08
IGP1 = 8.5e-7
TGHT = 270 A, 4.18 V
Omega 1375 °C, filament 1400 °C
The system stayed at those conditions for 15min
Thursday, August 15, 2024, 14:11
Ramping to 0A at 2A/min
|
Wednesday, August 07, 2024, 15:37, Aaron Schmidt, , , , , Turning on EVAP2's turbo pump
|
Wednesday, August 07, 2024, 15:36: Roughing. Had initially been roughed & TP started w/ Marla CS, however it timed out. Restarting.
Wednesday, August 07, 2024, 15:37: TP on.
Wednesday, August 07, 2024, 15:46: Tripped at 4 KRPM. Restarted. Up to 5 KRPM.
Failed to start.
Thursday, August 08, 2024, 10:00: TP started.
Thursday, August 08, 2024, 10:12: TP Tripped but nearly spun up. Reset & Restarted. TP Green / on. |
Thursday, August 08, 2024, 11:17, Marla Cervantes, C, 44139-5 SK, LP TUBE, Done, Graphite foils conditioning
|
Aaron Schmidt wrote: |
Wednesday, August 07, 2024, 15:36: Roughing. Had initially been roughed & TP started w/ Marla CS, however it timed out. Restarting.
Wednesday, August 07, 2024, 15:37: TP on.
Wednesday, August 07, 2024, 15:46: Tripped at 4 KRPM. Restarted. Up to 5 KRPM.
Failed to start.
Thursday, August 08, 2024, 10:00: TP started.
Thursday, August 08, 2024, 10:12: TP Tripped but nearly spun up. Reset & Restarted. TP Green / on.
|
Thursday, August 08, 2024, 10:43
A cartridge was filled with graphite foils and loaded in an uncoated tantalum tube. The tube was wrapped with four Ta-sheets. A Ta-foil was placed in the tube's right end for measuring the temperature.
Green graphite target characteristics
Number of discs |
822 |
Mass of discs |
11.74 g |
Mass of loaded cartridge with normal cap and hole-cap |
31.1290 g |
Mass of tube loaded, w/shields and tantalum cap |
250 g |
Note: A cartridge loaded with graphite foils has not been conditioned before. Thus, there is no reference on what current to use to reach 2000 °C.
The conditioning of a graphite composite target will be used as a reference, but note that the graphite foils are not expected to outgas as the composites since the foils do not contain binders and plasticizers.
Reference: Elog 636 Graphite inside insert Experiment 2 (regular formulation discs)
Initial ramps used in elog 636:
Currently waiting for vacuum to reduce to IGP1= 8.2e-07
Thursday, August 08, 2024, 11:23
Slope: 0.98 (same as slope used for tantalum targets since temperature is measured on Ta foil)
Friday, August 09, 2024, 08:50
Good vacuum 3e-5 Torr
Bad vacuum 5e-5 Torr
Initial IGP1 = 5.06E-7 Torr
Starting ramp at 1A/min to 200 A
Friday, August 09, 2024, 09:40 Pressure started to rise, but temperature is not within pyrometer range yet. Current 42 A, Voltage 0.5 V
Friday, August 09, 2024, 10:46 Pressure started to reduce (peak 1.4e-5 Torr). Temperature is not within pyrometer range yet Current 100 A, Voltage 1.3 V
Friday, August 09, 2024, 11:28 Temperature started to be detected, but not stable enough. Current 135 A, Voltage 1.9 V
Friday, August 09, 2024, 12:54 Temperature 1129 °C, current 196 A, voltage 3 V.
Friday, August 09, 2024, 12:56
Next ramp 0.5A/min while taking temperature readings periodically until 250A
Friday, August 09, 2024, 14:45
IGP1 = 1.0e-6 Torr
Next ramp 1A/min to 480 A aiming at 2000 °C
Friday, August 09, 2024, 17:13
IGP1 = 1.9e-6 Torr, Current 327A, Voltage 5.3V
Ramp changed to 2A/min to 480 A aiming at 2000 °C
Coolded down after 4 hours at ~2000°C
at -2A/min |
Thursday, July 25, 2024, 15:46, Angelina Chen, np-Ta, , TARGET BOAT, In progress, Carbonization of Heat Stabilized np-Ta Fibres Disk (1st Attempt)
|
Thursday, July 25, 2024, 15:18
Target container consists of two np-Ta fibres disk samples. Both disks are made from heat stabilized np-Ta fibres (150 C for 17 hours) and were pressed at 8 tons / 300 MPa.
Sample 1 was made from np-Ta fibres spun using Dope solution #1. Sample 1 disk has an average thickness of 0.727 mm and a diameter of 17.113 mm. Mass of the green sample 1 disk is 0.1957 g.
Sample 2 was made from np-Ta fibres spun using Dope solution #6. Sample 2 disk has an average thickness of 0.688 mm and a diameter of 17.123 mm. Mass of the heat stabilized fibres used to make the green sample 2 disk is 0.1860 g. Mass loss from pressing the heat stabilized fibres was virtually zero. Therefore, although the mass of the green sample 2 disk was not measured, it can be extrapolated to be 0.1860 g.
Target container was wrapped with Ta foil. Each sample disk was wrapped in graphite foil and placed inside the target container horizontally near the center.
Omega slope was initially set to 0.980. After reviewing previous logbook on np-Ti (e-log ID#633), changed the Omega slope to 0.990.
Chamber is currently being pumped down. The current reading (as of 15:40) is 4.70e-05 Torr.
Two heating schedules will be tested. Heating schedule 1 entails heating both sample disks at ~1000 C until the pressure reaches below 1.00e-06 Torr. Once heating schedule 1 is completed, sample 1 will be removed. Heating schedule 2 entails heating sample 2 to ~1800 C until the pressure reaches below 1.00e-06 Torr. TGHT is estimated to be approximately 440A/7.6V to reach 1875 C (348A/5.8V to hold temperature at 1600 C). Refer to e-log ID#605.
|
Friday, July 26, 2024, 10:05, John Wong, np-Ta, , TARGET BOAT, Done, Carbonization of Heat Stabilized np-Ta Fibres Disk (1st Attempt)
|
Angelina Chen wrote: |
Thursday, July 25, 2024, 15:18
Target container consists of two np-Ta fibres disk samples. Both disks are made from heat stabilized np-Ta fibres (150 C for 17 hours) and were pressed at 8 tons / 300 MPa.
Sample 1 was made from np-Ta fibres spun using Dope solution #1. The sample 1 disk has an average thickness of 0.727 mm and a diameter of 17.113 mm. The mass of the green sample 1 disk is 0.1957 g.
Sample 2 was made from np-Ta fibres spun using Dope solution #6. The sample 2 disk has an average thickness of 0.688 mm and a diameter of 17.123 mm. The mass of the heat stabilized fibres used to make the green sample 2 disk is 0.1860 g. The mass loss from pressing the heat stabilized fibres was virtually zero. Therefore, while the mass of the green sample 2 disk was not measured, it can be extrapolated to be 0.1860 g.
The target container was wrapped with Ta foil. Each sample disk was wrapped in graphite foil and placed inside the target container horizontally near the center.
The Omega slope was initially set to 0.980. After reviewing previous logbook on np-Ti
The chamber is currently being pumped down. The current reading (as of 15:40) is 4.70e-05 Torr.
Two heating schedules will be tested. Heating schedule 1 entails heating both sample disks at ~1000 C until the pressure reaches below 1.00e-06 Torr. Once heating schedule 1 is completed, sample 1 will be removed. Heating schedule 2 entails heating sample 2 to ~1800 C until the pressure reaches below 1.00e-06 Torr. TGHT is estimated to be approximately 440A/7.6V to reach 1875 C (348A/5.8V to hold temperature at 1600 C). Refer to e-log ID#605.
|
Friday, July 26, 2024, 09:52
Chamber has been pumped down overnight, pressure currently at 1e-6 Torr.
Initiate auto ramping 1A/min to reach 200 A.
Good vac = 3 e-5 Torr
Bad vac = 5 e-5 Torr.
Continue to monitor.
Friday, July 26, 2024, 17:06
Gas evolution has seen observed to be completed as TGHT slowly ramping up. Temp is currently reading at 1015 C, TGHT 164A/2.43V. Pressure holding at 2.4e-6 Torr but slowly coming down, see attachment 1. Will keep this setting and cool it down on Sunday.
Sunday, July 28, 2024, 11:27
Temperature has been holding sturdy at ~1000C for over 36 hours, TGHT at 164A/2.59V (a slight increase in the voltage). Pressure is currentlyat 4.5e-7 Torr (see attachment #2 for the archiver).
Ramping down TGHT at 1A/min.
Will remove both samples on Monday to measure the mass loss. Sample 1 will be analyzed. Sample 2 will be loaded back to the Evap 2 for further heating to reach about 1800 C.
Monday, July 29, 2024, 14:29
Both samples were removed from the chamber and measured for weight loss, and Sample 2 was put back for further heating; Thanks Darwin for helping up with this.
Chamber is currently pump down, pressure at 6.0e-5 Torr. Will ramp up TGHT once the pressure has come down to 10e-6 Torr.
Monday, July 29, 2024, 16:52
Pressure at 6.5e-6 Torr. Ramping up TGHT at 2A/min to reach 164A (previous setting at ~1000C).
Tuesday, July 30, 2024, 09:02
Temperature has been holding at about 1000C. THGT at 160A(readback,, 164A setpoint)/2.56V. Pressure 7e-7 Torr.
Stepping up 1A/min in 20A increment to reach 1800C.
Continue to monitor.
Tuesday, July 30, 2024, 10:07
Plotting out THGT (readback) vs Temp:
181 A/2.91V, 1070C
206A/3.34V, 1153C
225A/3.7V, 1213C
245A/4.1V, 1277C
Wednesday, July 31, 2024, 11:26
TGHT tripped off due to HS water flow NOT oK, Attempted to clear it but did not work, see attachment #3.
Will stop the process for now and investigate the problem.
Wednesday, July 31, 2024, 12:10
Darwin helped to check the surrounding of the lab for water leaks; everything was good and the chamber remained under vacuum.
All the water paddle wheels were moving. A slight touch of the HS paddle wheel somehow cleared the interlock. Maybe the connection was loose.
We checked all the paddle wheels by shutting and opening the water valves. All the interlocks responded correctly.
Continue with the heating process...
Ramping up TGHT at 2A/min to reach 300A.
Wednesday, July 31, 2024, 15:27
TGHT vs temp:
294A/5.1V 1477C
343A/6.0A, 1633C
402A/7.2V, 1818C
Will keep TGHT at 410A (setpoint) for night.(see attachment#4)
Tuesday, August 06, 2024, 10:00
Venting Evap 2; the process is done.
The sample will be analyzed.
|
Monday, July 22, 2024, 14:59, Aaron Schmidt, Ta, 45447-14, LP-SIS, In progress, Conditioning Ta#67 Thin foil
|
Ta#67 Thin foil LP-SIS target description:
Total Ta foils = 470 loaded into 2 packs of 235 foils each.
Foil Thickness = 0.010mm (0.0004") avg Measured.
Target material batch: https://elog.triumf.ca/TIS/Target+Production/143
Target density = 4.498 g/cm3
Target length = 3.7465 cm
Total Mass = 16.8509 g [Incl foils + Ta wire on 2 packs]
Total mass w/ Target oven = 415g (No end caps)
Discs in target are arranged as follows: 2packs
Dimpling direction on foils/ Packs. --> Center <--
No Ta foil heat shield added
Monday, July 22, 2024, 14:53: Roughing.
Halt roughing. Install heat plates.
Monday, July 22, 2024, 15:06: Roughing.
Monday, July 22, 2024, 15:26: TP On.
Monday, July 22, 2024, 15:34: TP Timeout. Restart.
Monday, July 22, 2024, 15:35: TP at speed (Green)
Monday, July 22, 2024, 15:36: PS On. TGHT / TBHT to 5/5 A manually. OK. Tap down.
Tuesday, July 23, 2024, 07:03: Auto-ramping TGHT / TBHT to 120 / 60 A @ 2 A per min. Desired temperature 1900 C.
Tuesday, July 23, 2024, 08:02: OMEGA IR2C Laser off. Slope set to 0.98.
Tuesday, July 23, 2024, 08:06: Auto-ramping TGHT / TBHT to 300 / 150 A @ 2 A per min.
Tuesday, July 23, 2024, 09:57: Auto-ramping TGHT / TBHT to 500 / 200 A @ 2 A per min. Temperature @ 1022 C.
Tuesday, July 23, 2024, 11:59: Auto-ramping TGHT / TBHT to 580 / 230 A @ 2 A per min. Temperature @ 1538 C.
Tuesday, July 23, 2024, 12:46: TGHT / TBHT @ 580 / 230 A (569 / 233 A). Temperature @ 1710 C. Vacuum @ 7.44e-06T.
Tuesday, July 23, 2024, 14:23: TGHT / TBHT @ 580 / 230 A (568 / 233 A). Auto-ramping TGHT to 620 A @ 2 A per min. Temperature @ 1721 C. Vacuum @ 5.06e-06T.
Tuesday, July 23, 2024, 14:48: TGHT / TBHT @ 620 / 230 A 609 / 233 A). Auto-ramping TGHT to 630 A @ 2 A per min. Temperature @ 1799 C. Vacuum @ 6.76e-06T.
Tuesday, July 23, 2024, 14:56: TGHT / TBHT @ 630 / 230 A 618 / 233 A). Temperature @ 1816 C. Vacuum @ 7.14e-06T. Tapping up manually TGHT to get to 1900degC
Tuesday, July 23, 2024, 15:23: TGHT / TBHT @ 670 / 230 A 657 / 233 A). Temperature @ 1890 C. Vacuum @ 9.94e-06T. Stopping and waiting for 5min.
Tuesday, July 23, 2024, 15:39: Target ramp down 2A/min to 0 both TGHT and TBHT.
Wednesday, July 24, 2024, 08:50: TP off.
Wednesday, July 24, 2024, 09:18: Venting.
Wednesday, July 24, 2024, 10:28: Target removed. EVAP2 clear. |
Wednesday, June 05, 2024, 07:18, Darwin Ortiz Rosales, SiC, , LP TUBE, Done, sinterin experiment 240604
|
Wednesday, June 05, 2024, 07:14
SiC discs loaded into tantalum tube. New mixing (two types) and old mixing.
The coated container tube was wrapped in four Ta foil heatshields.
Tac Coated springs at the ends in case plugs are pushed outwards.
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:=* 0.980*
Target time at max temperature = 4 hours
Final TGHT current= ~400A (adjustable)
Heating autoramp 1A/min to 90 A
Then at 2A/min to 120A.
Good vacuum = 5.0 e-02 Torr
Bad vacuum = 5.0E-04 Torr
IGP1 initia1.3e-06Torr
Wednesday, June 05, 2024, 11:04
Continuing to ramp at 2A/min to 350A
Wednesday, June 05, 2024, 12:22
Leaving at 369 A for 4 hours (until 4 pm). Temperature readings do not appear good.
Wednesday, June 05, 2024, 16:01
Start rampdown at -2A/min
IGP1=2.0 e-6 Torr |
Wednesday, May 29, 2024, 22:55, Darwin Ortiz Rosales, SiC, , LP TUBE, Done, Repeat of SiC experiment with mixed only casts
|
Wednesday, May 29, 2024, 22:52
Small graphite cartridge was loaded with SiC discs 240523-1 and 240523-2 and 220727-2 (baseline discs). Test Discs produced without milling using PAA as a dispersant.
The coated container tube was wrapped in four Ta foil heatshields.
two Tac Coated springs at the ends in case plugs are pushed outwards.
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final TGHT current= ~400A (adjustable)
Heating autoramp 2A/min to 90 A
Then at 2A/min to 120A.
Good vacuum = 5.0 e-02 Torr
Bad vacuum = 5.0E-04 Torr
IGP1 initial 4.8e-07 Torr
Wednesday, May 29, 2024, 22:54
Kept at 400 A for 4 hours.
Starting autoramp down at -2A/min
|
Monday, May 27, 2024, 07:12, Darwin Ortiz Rosales, SiC, , LP TUBE, Done, SiC (PAA dispersant experiment)
|
Monday, May 27, 2024, 07:09
Small graphite cartridge was loaded with SiC discs 240523-1 and 240523-2. Discs produced without milling using PAA as a dispersant.
The coated container tube was wrapped in four Ta foil heatshields.
two Tac Coated springs at the ends in case plugs are pushed outwards.
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final TGHT current= ~400A (adjustable)
Heating autoramp 2A/min to 90 A
Then at 2A/min to 120A.
Good vacuum = 5.0 e-02 Torr
Bad vacuum = 5.0E-04 Torr
IGP1 initial 4.8e-07 Torr
Monday, May 27, 2024, 09:13
Pressure started coming down. Heat at 2A/min to 120A.
Monday, May 27, 2024, 10:21
Started ramp 2A/30s to 400A will monitor temperature
stopped at 490A and will hold for 4 hours.
Monday, May 27, 2024, 12:41
temperature started creeping up past 1870C so decreased current to 461A
Current temperature is 1842 C at 461A, 7.6V
Monday, May 27, 2024, 12:55
dropped current to 441 because temperature climbed to 1899 C
Monday, May 27, 2024, 15:08
final pressure IGP1 =9.9 e-07 Torr
OMEGA= 1830 C at 410 A (reduced as needed)
Start rampdown at -2A/min
Wednesday, May 29, 2024, 10:07
Final pressure is 2.7e-7 Torr
Wednesday, May 29, 2024, 14:42
Experiment failed. Too hot probably. Bad temperature readings. Will repeat after redesigning experiment. |
Tuesday, May 07, 2024, 06:20, Darwin Ortiz Rosales, TaC, , TARGET BOAT, Done, Sintering TaC coating on endcaps
|
Tuesday, May 07, 2024, 06:16
TP was swapped on previous day (May 6th)
protective screen installed.
Loaded 9 TaC coated end caps (groups of 4 and 5) and 2 TaC coated springs.
OMEGA Slope 0.99
Will heat to 1850-1900 C and hold for 4 hours
Good Vac = 5.0e-4 Torr
Bad Vac= 5.0 e-02 Torr
Initial IGP1=6.7E-07 Torr
|
Wednesday, May 01, 2024, 11:54, Darwin Ortiz Rosales, TaC, 25447-27, HP-SIS, Done, TaC coating sintering
|
Wednesday, May 01, 2024, 11:53
The coated container was wrapped in 4 Ta foil heatshields.
Vacuum IGP1 initial =8.1 e-06 Torr
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230 A
Final TGHT current= ~500A (adjustable)
Heating autoramp starged at 3A/min(1A/30s) on TGHT 100A
Then at 2A/min to =400 A TGHT and 230A TBHT
Good vacuum = 5.0 e-04 Torr
Bad vacuum = 5.0E-02 Torr
Wednesday, May 01, 2024, 22:19
1830C reached at 670A. 10.0V TGHT
Start cooling after 4 hours. |
Friday, April 26, 2024, 06:19, Darwin Ortiz Rosales, TaC, 45447-29, HP-SIS, Done, TaC coating sintering
|
Monday, April 29, 2024, 19:50
Started coating with coating stand.
The coated container was wrapped in 3 Ta foil heatshields.
Vacuum IGP1 initial =9.1 e-07 Torr
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230 A
Final TGHT current= ~700A (adjustable)
Heating autoramp starged at 2A/min(1A/30s) on TGHT 100A
Then at 2A/min to =700 A TGHT and 230A TBHT
Good vacuum = 5.0 e-04 Torr
Bad vacuum = 5.0E-02 Torr
Monday, April 29, 2024, 20:25
Reached 1810 @700A
Will leave until 1230am |
Thursday, April 04, 2024, 12:07, Darwin Ortiz Rosales, TiC, , LP TUBE, Done, 240404TiC sintering/conditioning
|
Thursday, April 04, 2024, 12:06
Ta container tube, wrapped in 4 Ta foil heat-shields, and loaded with _________ D shaped discs in a 12mm graphite cartridge with usable 11mm
conditioning tube WO = 44692-13 (4th conditioning with this tube)
End-caps on the graphite cartridge have holes for outgassing. One spring each end in the Ta container
initial heating @ 2A/min to 85 A then 2A/min to 120A TGHT
OMEGA slope = 0.99
Vacuum limits up to 400A: 5.0e-04 Torr -- 1.0e-02 Torr
Mas current~400A (1900 C)
Friday, April 05, 2024, 09:04
Ramping to 85A done and pressure trending down. Will continue ramp to 120A
Friday, April 05, 2024, 16:01
Starting rampdown at -2A/min
IGP1= 3.2e-06 Torr
|
Wednesday, April 03, 2024, 06:46, Darwin Ortiz Rosales, TiC, , LP TUBE, Done, 240402TiC
|
Wednesday, April 03, 2024, 06:46
Ta container tube, wrapped in 4 Ta foil heat-shields, and loaded with _________ D shaped discs in a 12mm graphite cartridge with usable 11mm
conditioning tube WO = 44692-13
End-caps on the graphite cartridge have holes for outgassing. One spring each end in the Ta container
initial heating @ 2A/min to 85 A then 2A/min to 120A TGHT
OMEGA slope = 0.99
Vacuum limits up to 400A: 5.0e-04 Torr -- 1.0e-02 Torr
Wednesday, April 03, 2024, 06:49
initial IGP1= 1.28e-06 Torr
Wednesday, April 03, 2024, 09:26
IGP1= 2.3e-05 Torr
TGHT = 78 A, 1.3V
Will continue ramp as planned.
Wednesday, April 03, 2024, 11:37
Ramping at 2A./min to 400A
Wednesday, April 03, 2024, 14:01
expected 1900C at 401A
leaving at 402A for 4 hours. Rampdown start at 4:10 pm at -2A/min |
Thursday, February 29, 2024, 07:40, Darwin Ortiz Rosales, TiC, , LP TUBE, Done, 240228TiC conditioning
|
Thursday, February 29, 2024, 07:40
Ta container tube, wrapped in 4 Ta foil heat-shields, and loaded with _________ D shaped discs in a 12mm graphite cartridge with usable 11mm
conditioning tube WO = 44692-13
End-caps on the graphite cartridge have holes for outgassing. One spring each end in the Ta container
initial heating @ 2A/min to 85 A then 2A/min to 120A TGHT
OMEGA slope = 0.99
Vacuum limits up to 400A: 5.0e-04 Torr -- 1.0e-02 Torr
Thursday, February 29, 2024, 07:43
Initial IGP1= 9.31e-7 Torr
Thursday, February 29, 2024, 17:43
Temperature profile suggests 1900 C at 400A. Now at 400A. Will keep at this current for 4 hours.
manually ramped the last few amps.
TGHT= 400A, 7.3 V OMEGA = 1901C
Thursday, February 29, 2024, 22:20
IGP1=2.1e-6 Torr
started ramping down at -2A/min
|
Wednesday, February 21, 2024, 06:23, Darwin Ortiz Rosales, TiC, , LP TUBE, Done, 240220TiC conditioning
|
Wednesday, February 21, 2024, 06:22
Ta container tube, wrapped in 4 Ta foil heat-shields, and loaded with 201 D shaped discs in a 12mm graphite cartridge with usable 11mm
conditioning tube WO = 44692-13
End-caps on the graphite cartridge have holes for outgassing. One spring each end in the Ta container
initial heating @ 2A/min to 90 A then 1A/min to 120A TGHT
OMEGA slope = 0.99
Vacuum limits up to 400A: 5.0e-04 Torr -- 1.0e-02 Torr
Wednesday, February 21, 2024, 09:12
IGP1 initial = 9e-07 Torr
Starte at 3A/min to 90A
Wednesday, February 21, 2024, 09:21
increased autoramp to 4 A/min until pressure starts rising, then will slow down or pause
Wednesday, February 21, 2024, 09:32
At 74A, paused. Will continue at 2A/min TGHT
Wednesday, February 21, 2024, 09:40
Pausing at 87A.
Wednesday, February 21, 2024, 10:34
pressure dropping. restarting ramp up to 120A at 2A/min
Wednesday, February 21, 2024, 10:37
From previous TiC 220206, will heat up fast until 250A and then at 1A/min until 300A to better resolve out-gassing profile
Wednesday, February 21, 2024, 12:05
Changed ramp to 1A/min to 300A
Wednesday, February 21, 2024, 13:10
Manually ramped up for a while
increased ramp speed to 2A/min
regression line started to match previous one after 1300C
Wednesday, February 21, 2024, 13:16
increased ramp rate to 4A/min to 420A
Wednesday, February 21, 2024, 13:37
Note: the temperature became unrealistic. suspect window condensate. Will use regression and to to 441A
Wednesday, February 21, 2024, 13:54
reached 441A, 7.6V
leaving for 3.5 hours or when pressure drops to 2-3 e-06 Torr
Wednesday, February 21, 2024, 18:56
IGP1=2.9e-06 Torr
starting rampdown at -2A/min |
Wednesday, February 07, 2024, 22:49, Darwin Ortiz Rosales, TiC, 44692-11, LP TUBE, Done, 240206TiC conditioning
|
Wednesday, February 07, 2024, 22:36
Ta container tube TaC coated, wrapped in 4 Ta foil heat-shields, and loaded with 320 D shaped discs in a 12mm graphite cartridge with usable 11mm
Endcaps on the graphite cartridge have holes for outgassing
initial heating @ 2A/min to 90 A then 1A/min to 120A TGHT
OMEGA slope = 0.99
Vacuum limits up to 400A: 5.0e-04 Torr -- 1.0e-02 Torr
Thursday, February 08, 2024, 06:18
Starting heat ramp tght
initial pressure = 8.1e-07 Torr IGP1
Thursday, February 08, 2024, 06:54
start of gasoff observed. paused ramp and will continue at 1A/min
Thursday, February 08, 2024, 07:24
lowered TGHT current to 75 A as pressure increasing too rapidly. will leave at this current until pressure drops
Thursday, February 08, 2024, 09:11
continuing ramp to 120A on TGHT
Thursday, February 08, 2024, 09:24
Increasing ramp to 2A/min to 250A on TGHT
Thursday, February 08, 2024, 10:52
Increased ramp to 3A/min to 250A on TGHT
Thursday, February 08, 2024, 11:10
Everything looks good will continue to 300 A at 3A/min TGHT
Thursday, February 08, 2024, 11:33
Pausing heating at 285A, 4.8V TGHT
OMEGA reads 1430C
Will let pressure drop and then proceed ramping slowly @ 0.2A/min
Thursday, February 08, 2024, 13:53
IGP1= 2.4e-06 Torr
OMEGA = 1432 C
ramp at 0.2A/min towards 1550C
Thursday, February 08, 2024, 14:07
pressure very stable. will increase to 0.4 A/min
Thursday, February 08, 2024, 15:24
increasing ramp rate to 1A/min
IGP1 = 2.5e-06 Torr
Thursday, February 08, 2024, 18:05
1900 C on OMEGA
will leave 3-4 hours depending on pressure
Thursday, February 08, 2024, 21:10
No additional pressure peaks observed and pressure on IGP1= 1.9e-06 Torr
TGHT= 460 A, 8.1V
OMEGA= 1860 C
ramp down at -2A/min
|
Monday, January 29, 2024, 16:45, Darwin Ortiz Rosales, TaC, , LP-FEBIAD, Done, TaC coating sintering
|
Monday, January 29, 2024, 16:36
LP FEBIAD
wrapped in 4 Ta heatshields.
Will heat at 2A/min to 95A on TGHT and TBHT
Then will heat at 3A/min to 1800 C ~400A on TGHT and 230A on TBHT
Monday, January 29, 2024, 16:45
Initial IGP1= 5e-05 Torr
Monday, January 29, 2024, 20:35
1800C was at TGHT 410A, 6.9V RD and set current 418A
TBHT= 233 RD A, 3.2V
|
Friday, January 26, 2024, 07:06, Darwin Ortiz Rosales, TaC, 45447-1, HP-FEBIAD, Done, TaC coating sintering
|
Friday, January 26, 2024, 07:05
The coated container was wrapped in 4 Ta foil heatshield and left in evap2 over night to attain vacuum.
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230 A
Final TGHT current= ~700A (adjustable)
Heating autoramp starged at 1A/min on TGHT and TBHT to 120A
Then at 2 A/min to =400 A TGHT and 230A TBHT
Good vacuum = 5.0 e-04 Torr
Bad vacuum = 5.0E-02 Torr
Initial IGP1= 5.7e-05 Torr
Friday, January 26, 2024, 09:20
Pressure starts increasing at 125 A on TGHT and TBHT. Leaving it to equilibrate then will start ramping at 3A/min (1.5A/30s) to 700A on TGHT and 230A on TBHT
Friday, January 26, 2024, 13:18
leave sintering at 1838C . Will start rampdown at 5 pm.
IGP1= 6.10e-06 Torr
TGHT=680A, 10.14V
TBHT = 230A, 3.13V
Friday, January 26, 2024, 16:52
IGP1 = 3.0e10-6 Torr
OMEGA=1821 C
start rampdown @-2A/min TGHT and -1A/min TBHT |
Thursday, December 14, 2023, 09:58, Darwin Ortiz Rosales, SiC, 41369-2, HP-SIS, Done, 231208SiC conditioning
|
Thursday, December 14, 2023, 09:53
Target left pumping down in Evap2 overnight.
Initial weight including protective jig = 1474.3 g
Total number of target foils:388
10 analysis discs: 5x 220727-2 labelled as A and 5x 231123-2 labelled as B on the right side (front) of container. Order of discs ABABABABAB.
Total length packed 15.5 cm
container has 3 Ta heat shields including the inner made of three pieces as to cover the center block.
No endcaps inserted to facilitate out-gassing
Ta coated spring at both ends
ramp to 500A @ 1A/min TGHT and to 230A on TBHT
max approx 700A on TGHT and 230A on TBHT (Omega slope set = 0.990)
Then temperature = 1800C
TBHT will be set fixed at 230 A (max). TBHT heated manually and automatically to max.
Good vac at 5.00 e -4 Torr
Bad vac at 5.00 e-2 Torr
IGP1= 9.3e-07 Torr at start of initial ramp.
Thursday, December 14, 2023, 09:56
Started initial ramp up 1A/min on both heaters
Thursday, December 14, 2023, 11:03
Pressure dropping. Will increase ramp speed to 2A/min on both heaters (1A/30s)
Thursday, December 14, 2023, 11:17
pressure dropping. Increase ramp to 4A/min (2A/30s)
Will stop and ramping for temperature measurements
Thursday, December 14, 2023, 13:28
Increased ramp to 5A/min (2.5A/30s)
Will heat to 703A on TGHT and leave for 4 hours |
Wednesday, December 06, 2023, 09:57, Darwin Ortiz Rosales, SiC, 45447-4, HP-FEBIAD, Done, 231204SiC conditioning
|
Wednesday, December 06, 2023, 09:47
Target number of foils:370
Analysis discs 16 A and 16B interspersed on the end further from the laser
A are discs produced using new method and B are discs produced using milling.
Total length packed 16 cm (excluding the analysis discs)
container has 3 Ta heat shields (one inner around fins and center block, new type of 1st shield made up of three pieces)
No endcaps inserted to facilitate out-gassing
Ta coated spring at front end
ramp to 120A @ 1A/min TGHT and to 120A on TBHT hold there until pressure drop, then ramp to 500A on TGHT and 230A TBHT.
max approx 700A on TGHT and 230A on TBHT (Omega slope set = 0.990)
Then temperature = 1800C
TBHT will be set fixed at 230 A (max). TBHT heated manually and automatically to max.
Good vac at 5.00 e -4 Torr
Bad vac at 5.00 e-2 Torr
IGP1= 1e-06 Torr at start of initial ramp.
Wednesday, December 06, 2023, 09:56
System left to drop pressure over previous night and now at 120A. waiting for pressure drop.
Wednesday, December 06, 2023, 11:18
increased ramp rate to 2A/min
Wednesday, December 06, 2023, 14:41
increased ramp to 3A/min on TGHT and stopping to allow pressure to stabilize before taking temperature readings
Top temperature 1800C at 710 A but started dropping. Increased current to 750A and left there for 4 hours.
Cool down at -2A/min TGHT and -1A/min TBHT
|
Monday, November 06, 2023, 14:07, Darwin Ortiz Rosales, Empty, 45220-4, LP-SIS, Done, TaC coating sintering
|
Monday, November 06, 2023, 09:59
The coated container was wrapped in 4 Ta foil heatshields.
Vacuum IGP1 initial =3.1 e-07 Torr
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230 A
Final TGHT current= ~400A (adjustable)
Heating autoramp starged at 2A/min(1A/30s) on TGHT 100A
Then at 2A/min to =400 A TGHT and 230A TBHT
Good vacuum = 5.0 e-04 Torr
Bad vacuum = 5.0E-02 Torr
Monday, November 06, 2023, 14:07
OMEGA =1852 C
IGP1= 3.14e-06 Torr
TGHT= 399A, 6.6V
TBHT= 233A, 4.1V
Tuesday, November 07, 2023, 12:28
Cooled down previous evening and took out today.
rampdown was @-2A/min for TGHT and -1A/min TBHT |
Friday, October 20, 2023, 07:24, Darwin Ortiz Rosales, TaC, 45447-11, LP-SIS, Done, TaC coating sintering
|
Friday, October 20, 2023, 07:20
The coated container was wrapped in 4 Ta foil heatshields.
Vacuum IGP1 initial = 9.9 e-07 Torr
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230 A
Final TGHT current= ~400A (adjustable)
Heating autoramp starged at 2A/min(1A/30s) on TGHT 100A
Then at 4A/min to =400 A TGHT and 230A TBHT
Good vacuum = 5.0 e-04 Torr
Bad vacuum = 5.0E-02 Torr
Friday, October 20, 2023, 07:24
Starting initial ramp
Vacuum IGP1 initial = 9.9 e-07 Torr
Friday, October 20, 2023, 08:55
After initial pressure bump continued heating at 1A/min to 120A to observe any other possible pressure bump.
Friday, October 20, 2023, 09:05
increased ramp to 4A/min to 400 TGHT and 230 TBHT
Friday, October 20, 2023, 09:35
OMEGA=1280 C
TGHT= 221.5 A, 3.24V
TBHT=228.9, 3.9V
Friday, October 20, 2023, 10:22
OMEGA 1852 C at TGHT = 390A, 6.5 V ; TBHT = 232 A, 4.0 V
Will leave for 4 hours
Friday, October 20, 2023, 14:16
About to start rampdown
TGHT @ -2A/min
TBHT@ -1A/min
Final OMEGA = 1840 C
IGP1 = 1.83e-06 Torr |
Thursday, October 05, 2023, 12:47, Aaron Schmidt, Ta, 45220-3, LP-SIS, In progress, Conditioning Ta#68 (Spare)
|
Ta#(Spare) LP-SIS target description:
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.033mm (0.0013") avg Measured.
Target material batch: Ta 2023-1 Mt'l PO# TR-2022-03028
Target density = 12.515 g/cm3
Target length = 4.97 cm
Total Mass = 62.202 g [Incl foils + Ta wire on 6 packs]
Total mass w/ Target oven = 461g (w/ end caps)
Discs in target are arranged as follows: 1pack / 75 singles / 1pack / 100 singles / 2packs / 100 singles / 1pack / 75 singles / 1pack
Dimpling direction on foils/ Packs. --> Center <--
End caps installed (Not expanded). No Ta foil heat shield added
Was labelled Ta#67 until the Thin foil target 45447-14 became so.
Thursday, October 05, 2023, 12:44: Roughing.
Thursday, October 05, 2023, 13:10; TP1 on.
Thursday, October 05, 2023, 13:11: TGHT / TBHT test. Tap up to 5 / 5 A & back to 0 A. Ok.
Thursday, October 05, 2023, 13:13: Slope Set @ 0.98
Friday, October 06, 2023, 05:54: Auto-ramping TGHT / TBHT to 580 / 230 A @ 2 A per min.
Friday, October 06, 2023, 11:50: TGHT / TBHT @ 580 / 230 A (568 / 233 A). Auto-ramping TGHT to 630 A @ 2 A per min (640 A w/ offset). Temperature @ 1716 C. Vacuum @ 2.76e-06T.
Friday, October 06, 2023, 12:20: TGHT / TBHT @ 630 / 230 A (618 / 233 A). Auto-ramping TGHT to 650 A @ 2 A per min (640 A w/ offset). Temperature @ 1809 C. Vacuum @ 3.77e-06T.
Friday, October 06, 2023, 12:37: TGHT / TBHT @ 650 / 230 A (638 / 233 A). Auto-ramping TGHT to 665 A @ 2 A per min (650 A w/ offset). Temperature @ 1844 C.
Friday, October 06, 2023, 12:53: Tapped up to TGHT / TBHT @ 670/ 230 A (657 / 233 A). Temperature @ 1880 C. Vacuum @ 4.94e-06T.
Friday, October 06, 2023, 12:57: Tapped TGHT to 675. TGHT / TBHT @ 675 / 230 A (662 / 233 A). Temperature @ 1889 C. Vacuum @ 5.03e-06T.
Friday, October 06, 2023, 13:00: Tapped TGHT to 682. TGHT / TBHT @ 682 / 230 A (669 / 233 A). Temperature @ 1901 C. Vacuum @ 5.46e-06T. Desired Temperature reached.
Friday, October 06, 2023, 13:01: Auto-cooling @ 2 A per min.
Tuesday, October 10, 2023, 08:37: PS & TP off. |
Wednesday, September 20, 2023, 14:26, Aaron Schmidt, Ta, 45220-5, LP-SIS, In progress, Conditioning Ta#66
|
Ta#66 LP-SIS target description:
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.033mm (0.0013") avg Measured.
Target material batch: Ta 2023-1 Mt'l PO# TR-2022-03028
Target density = 12.446 g/cm3
Target length = 5.0 cm
Total Mass = 62.230 g [Incl foils + Ta wire on 6 packs]
Total mass w/ Target oven= g (w/ end caps)
Discs in target are arranged as follows: 1pack / 75 singles / 1pack / 100 singles / 2packs / 100 singles / 1pack / 75 singles / 1pack
Dimpling direction on foils/ Packs. --> Center <--
End caps installed (Not expanded). No Ta foil heat shield added
Desired temperature 1900C
Wednesday, September 20, 2023, 14:18: Roughing.
Wednesday, September 20, 2023, 14:35: TP Started.
Wednesday, September 20, 2023, 14:43: TP on.
Wednesday, September 20, 2023, 14:45: TGHT / TBHT raised to 5 / 5 A & lowered. Quick check ok.
Thursday, September 21, 2023, 07:47: Auto-ramping TGHT / TBHT to 580 / 230 A @ 2 A per min. Vacuum @ 8.30e-07T.
Thursday, September 21, 2023, 09:54: Slope set to 0.98
Thursday, September 21, 2023, 13:42: TGHT / TBHT @ 580 / 230 A (568 / 233 A). Auto-ramping TGHT to 630 A @ 2 A per min (640 A w/ offset). Temperature @ 1748 C. Vacuum @ 2.47e-06T.
Thursday, September 21, 2023, 14:10: TGHT / TBHT @ 630 / 230 A (618 / 233 A). Auto-ramping TGHT to 650 A @ 2 A per min (640 A w/ offset). Temperature @ 1843 C. Vacuum @ 3.30e-06T.
Thursday, September 21, 2023, 14:23: TGHT / TBHT @ 650 / 230 A (638 / 233 A). Auto-ramping TGHT to 660 A @ 2 A per min (648 A w/ offset). Temperature @ 1879 C. Vacuum @ 3.77e-06T.
Thursday, September 21, 2023, 14:29: Tapped TGHT to 662. TGHT / TBHT @ 662 / 230 A (649 / 233 A). Temperature @ 1903 C. Vacuum @ 4.08e-06T. Desired Temperature reached.
Thursday, September 21, 2023, 14:33: Auto-cooling started @ 1 A per min.
Monday, September 25, 2023, 08:09: Turbo pump off. |
Tuesday, September 12, 2023, 09:54, Darwin Ortiz Rosales, TaC, 41369-2, HP-SIS, Done, TaC coating sintering
|
Tuesday, September 12, 2023, 09:51
The coated container was wrapped in 3 Ta foil heatshield and left in evap2 over night to attain vacuum.
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230 A
Final TGHT current= ~700A (adjustable)
Heating autoramp starged at 1A/min on TGHT and TBHT to 120A
Then at 2 A/min to =400 A TGHT and 230A TBHT
Good vacuum = 5.0 e-04 Torr
Bad vacuum = 5.0E-02 Torr
Initial IGP1= 2.7e-06 Torr
Tuesday, September 12, 2023, 7:00
Started autoramp @1A/min to 120A on both TGHT and TBHT
Tuesday, September 12, 2023, 09:53
Heating ramp set to 230A for both TGHT and TBHT. Rate at 2A/min for both heaters.
Tuesday, September 12, 2023, 11:21
Continued ramp on TGHT at 2A/min to 335A and now setting to 3A/min (1.5A/30s)
Tuesday, September 12, 2023, 11:47
|
TGHT |
|
Temperature ( C ) |
Voltage (V) |
Current (A) |
1205 |
5.5 |
392.0 |
Continue ramping @3A/min on TGHT
Tuesday, September 12, 2023, 13:33
Reached 1840 C at TGHT =677A and 10.5V
Will keep for 4 hours |
Thursday, August 31, 2023, 07:09, Darwin Ortiz Rosales, TaC, 45447-4, HP-FEBIAD, Done, TaC coating sintering
|
Thursday, August 31, 2023, 07:07
The coated container was wrapped in 3 Ta foil heatshields.
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230 A
Final TGHT current= ~500A (adjustable)
Heating autoramp starged at 1A/min on TGHT and TBHT to 120A
Then at 2 A/min to =400 A TGHT and 230A TBHT
Good vacuum = 5.0 e-04 Torr
Bad vacuum = 5.0E-02 Torr
Initial IGP1= 7.7e-07 Torr
Thursday, August 31, 2023, 12:29
OMEGA=1238 C
IGP1=1.4e-06 Torr
Continue ramp
ramp @ 4A/min (2A/30s)
Thursday, August 31, 2023, 12:50
IGP1= 2.23e-06 Torr
OMEGA=1392 C
Thursday, August 31, 2023, 13:04
IGP1=2.7e-06 Torr
OMEGA=1443 C
Thursday, August 31, 2023, 13:18
IGP1= 3.8e-06 Torr
OMEGA=1537 C
Thursday, August 31, 2023, 14:38
OMEGA=1852C |
Tuesday, August 29, 2023, 12:47, Darwin Ortiz Rosales, TaC, 45220-10, LP-SIS, Done, TaC coating sintering
|
Tuesday, August 29, 2023, 12:46
The coated container was wrapped in 4 Ta foil heatshields.
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230 A
Final TGHT current= ~400A (adjustable)
Heating autoramp starged at 2A/min(1A/30s) on TGHT 100A
Then at 4A/min to =400 A TGHT and 230A TBHT
Good vacuum = 5.0 e-04 Torr
Bad vacuum = 5.0E-02 Torr
Tuesday, August 29, 2023, 12:49
Initial heating start
IGP1= 6.0 e-06 Torr
Tuesday, August 29, 2023, 14:31
Paused ramping to take reading
IGP1= 5.98e-06 Torr
OMEGA = 1500 C
Tuesday, August 29, 2023, 15:24
OMEGA 1866 C
IGP1= 6.6e-6 Torr
|
Saturday, August 26, 2023, 09:41, Darwin Ortiz Rosales, TaC, 45220-10, LP-SIS, Done, TaC coating sintering
|
Saturday, August 26, 2023, 09:39
The coated container was wrapped in 4 Ta foil heatshields.
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230 A
Final TGHT current= ~400A (adjustable)
Heating autoramp starged at 2A/min(1A/30s) on TGHT 100A
Then at 4A/min to =400 A TGHT and 230A TBHT
Good vacuum = 5.0 e-04 Torr
Bad vacuum = 5.0E-02 Torr
Initial IGP1= 8.7e-07 Torr
Saturday, August 26, 2023, 10:54
IGP1= 1.2e-06 Torr
Start ramp up at 4A/min on both heaters (2A/30s) until TGHT = 400A and TBHT=230A
Saturday, August 26, 2023, 11:32
Paused ramp to allow temperature to stabilize and record data
OMEGA= 1396 C
IGP1= 2.47e-06 Torr
Saturday, August 26, 2023, 11:52
Paused ramp to record data
OMEGA = 1544 C
IGP1=3.4e-06 Torr
Saturday, August 26, 2023, 12:09
Paused ramp to record data
OMEGA = 1653
IGP1 = 4.5e-06 Torr
Saturday, August 26, 2023, 12:33
Omega went up to 1878C. Lowered the current on TGHT to reach OMEGA = 1857 C
Will keep until 430 pm
IGP1- 3.4e-06 Torr
Saturday, August 26, 2023, 16:10
ramping down at -2A/min tght 1A/min tbht
1837 C OMEGA
|
Thursday, August 24, 2023, 14:18, Aaron Schmidt, Nb, 45447-9, LP-IG-LIS, In progress, Conditioning Nb#11
|
Nb#11 LP-IG-LIS target description:
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.025mm (0.001")
Target density = 7.13 g/cm3
Target length = 3.53 cm
Total Mass = 25.165 g [Incl foils + Ta wire on 6 packs]
Total mass w/ Target oven= 434 g (w/ end caps)
Discs in target are arranged as follows: 1pack / 75 singles / 1pack / 100 singles / 2packs / 100 singles / 1pack / 75 singles / 1pack
Dimpling direction on foils/ Packs. --> Center <--
End caps installed (Not expanded). No Ta foil heat shield added
Final desired temperature = 1900C.
Replacement for Nb#10
Thursday, August 24, 2023, 14:16: Roughing.
OMEGA slope = 0.98.
Thursday, August 24, 2023, 14:31: Turbo pump started.
Thursday, August 24, 2023, 14:41: TGHT / TBHT PS on. Manually test @ 5 / 5 A. ok. Tap back to 0 A.
Thursday, August 24, 2023, 18:26: Vacuum @ 4.35e-06T. Auto-ramping TGHT / TBHT to 580 / 230 A @ 2 A per minute.
Thursday, August 24, 2023, 22:00: TGHT / TBHT @ 414 / 230 A (406 / 233 A - Offset). Auto-ramping TGHT to 580 A @ 2 A per min continued. Temperature @ 1353 C. Vacuum @ 4.03e-06T.
Thursday, August 24, 2023, 23:29: TGHT / TBHT @ 580 / 230 A (569 / 233 A). Auto-ramping TGHT to 610 A @ 2 A per min (approx 600 A w/ offset). Temperature @ 1708 C. Vacuum @ 6.61e-06T.
Thursday, August 24, 2023, 23:49: TGHT / TBHT @ 610 / 230 A (598 / 233 A). Auto-ramping TGHT to 630 A @ 2 A per min (620 A w/ offset). Temperature @ 1765 C. Vacuum @ 7.22e-06T.
Friday, August 25, 2023, 00:04: TGHT / TBHT @ 630 / 230 A (618 / 233 A). Auto-ramping TGHT to 650 A @ 2 A per min (640 A w/ offset). Temperature @ 1808 C. Vacuum @ 7.54e-06T.
Friday, August 25, 2023, 00:16: TGHT / TBHT @ 650 / 230 A (638 / 233 A). Auto-ramping TGHT to 670 A @ 2 A per min (660 A w/ offset). Temperature @ 1845 C. Vacuum @ 7.72e-06T.
Friday, August 25, 2023, 00:27: TGHT / TBHT @ 670 / 230 A (657 / 233 A). Auto-ramping TGHT to 680 A @ 2 A per min (668 A w/ offset). Temperature @ 1880 C. Vacuum @ 8.46e-06T.
Manually tap up to temperature.
Friday, August 25, 2023, 00:34: TGHT / TBHT @ 682 / 230 A (669 / 233 A). Temperature @ 1900-1901 C. Vacuum @ 8.59e-06T. Desired Temperature Reached.
Friday, August 25, 2023, 00:37: Auto-cooling @ 2 A per min.
Friday, August 25, 2023, 06:15:
Friday, August 25, 2023, 07:40: PS & TP off.
|
Tuesday, August 22, 2023, 09:35, Darwin Ortiz Rosales, TaC, 44692-11, TARGET BOAT, Done, TaC coating sintering (second coating on same tube)
|
Tuesday, August 22, 2023, 09:29
The coated container was wrapped in 4 Ta foil heatshields.
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 2 hours
Final Current TBHT= N/A
Final TGHT current= ~400A (adjustable)
Heating autoramp starged at 2A/min(1A/30s) on TGHT 100A
Then at 4A/min to =400 A.
Good vacuum = 5.0 e-04 Torr
Bad vacuum = 5.0E-02 Torr
IGP1 initial =2.2e-06 Torr
Tuesday, August 22, 2023, 10:25
IGP1= 2.31e-06 Torr
TGHT 98.0 A (RD), 1.35 V
Start ramping at 2A/min to 400A
Tuesday, August 22, 2023, 11:54
Reached 1860 @ TGHT = 353A, 6.16V (RD) Will leave for 2 hours
Tuesday, August 22, 2023, 14:07
1853C OMEGA
TGHT = 353 A, 6.2 V (RD)
IGP1= 2.88E-06 Torr
Starting ramp-down at -2A/min
Saturday, August 26, 2023, 09:37
Note: the coating looks really good . The second sintering on the second coating was 2 hours. Will test the coating during graphite material conditioning. |
Tuesday, August 15, 2023, 12:03, Darwin Ortiz Rosales, TaC, 44692-11, TARGET BOAT, Done, TaC coating sintering
|
Tuesday, August 15, 2023, 10:48
The coated container was wrapped in 4 Ta foil heatshields.
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= N/A
Final TGHT current= ~400A (adjustable)
Heating autoramp starged at 2A/min(1A/30s) on TGHT 100A
Then at 4A/min to 100 A.
Good vacuum = 5.0 e-04 Torr
Bad vacuum = 5.0E-02 Torr
IGP1 initial =8.9e-06 Torr
Tuesday, August 15, 2023, 13:00
Tuesday, August 15, 2023, 13:00
Pressure stabilizing @8.8e-06 Torr
starting 2A/30s ramp to 400 A
Tuesday, August 15, 2023, 14:02
TGHT RD CURRENT = 331.4A, 5.8V, SET CURRENT=338 A.
OMEGA = 1855
IGP1= 1.5e-05 Torr
Leave for 4 hours
Tuesday, August 15, 2023, 15:05
Temperature dropped slightly to 1820C so increased current set point to 345A, and RD was at 338A, 5.9V
OMEGA increased to 1842C
Tuesday, August 15, 2023, 17:59
OMEGA = 1823C
TGHT= RD 338A, 5.9V SET= 345A
IGP1= 4.0e-06 Torr
Start rampdown at -2A/min |
Wednesday, June 21, 2023, 10:37, Aaron Schmidt, Nb, 45447-7, LP-IG-LIS, In progress, Conditioning Nb#10
|
Nb#10 LP-IG-LIS target description:
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.025mm (0.001")
Target density = 7.36 g/cm3
Target length = 3.5 cm
Total Mass = 25.7576 g [Incl foils + Ta wire on 6 packs]
Total mass w/ Target oven= 438 g (w/ end caps)
Discs in target are arranged as follows: 1pack / 75 singles / 1pack / 100 singles / 2packs / 100 singles / 1pack / 75 singles / 1pack
Dimpling direction on foils/ Packs. --> Center <--
End caps installed (Not expanded). No Ta foil heat shield added
Wednesday, June 21, 2023, 10:37: Roughing.
Wednesday, June 21, 2023, 13:39: TP1 on.
Wednesday, June 21, 2023, 13:55: TGHT / TBHT PS on. Vacuum @ 3.35e-05T
Thursday, June 22, 2023, 13:16: TGHT / TBHT Manually set to 5 / 5 A. Vacuum @ 8.17e-07T.
Final desired temperature = 1900C.
Thursday, June 22, 2023, 13:49: OMEGA slope = 0.98.
Friday, June 23, 2023, 06:24: Auto-ramping TGHT / TBHT to 580 / 230 @ 2 A per min.
Friday, June 23, 2023, 12:11: TGHT / TBHT @ 580 / 230 A (568 / 233 A). Auto-ramping TGHT to 610 A @ 2 A per min (600 A w/ offset). Temperature @ 1697 C. Vacuum @ 3.38e-06T.
Friday, June 23, 2023, 12:32: TGHT / TBHT @ 610 / 230 A (600 / 233 A). Auto-ramping TGHT to 630 A @ 2 A per min (620 A w/ offset). Temperature @ 1748 C. Vacuum @ 4.61e-06T.
Friday, June 23, 2023, 12:44: TGHT / TBHT @ 630 / 230 A (617 / 233 A). Auto-ramping TGHT to 650 A @ 2 A per min (640 A w/ offset). Temperature @ 1790 C. Vacuum @ 5.74e-06T.
Friday, June 23, 2023, 13:07: TGHT / TBHT @ 650 / 230 A (638 / 233 A). Auto-ramping TGHT to 670 A @ 2 A per min (660 A w/ offset). Temperature @ 1825 C. Vacuum @ 5.90e-06T.
Friday, June 23, 2023, 13:22: TGHT / TBHT @ 670 / 230 A (658 / 233 A). Auto-ramping TGHT to 680 A @ 2 A per min (668 A w/ offset). Temperature @ 1858 C. Vacuum @ 6.75e-06T.
Friday, June 23, 2023, 13:29: TGHT / TBHT @ 680 / 230 A (667 / 233 A). Auto-ramping TGHT to 690 A @ 2 A per min (677 A w/ offset). Temperature @ 1877 C. Vacuum @ 6.99e-06T.
Friday, June 23, 2023, 13:37: Manually tap up to temperature.
Friday, June 23, 2023, 13:38: Vacuum @ 7.54e-06T. TGHT / TBHT @ 694 / 230 A (680.5 / 233 A direct w/ offset). Temperature @ 1901-1902 C. Desired Temperature Reached.
Friday, June 23, 2023, 13:42: Auto-cooling @ 2 A per min. |
Thursday, June 08, 2023, 09:29, Darwin Ortiz Rosales, TaC, , TARGET BOAT, Done, TaC coated endcaps and spring sintering (new TaC)
|
Thursday, June 08, 2023, 09:28
Using smaller particle size TaC no ball mill procedure.
Loaded 2 TaC coated end caps and 1 TaC coated springs.
OMEGA Slope 0.99
Will heat to 1850-1900 C and hold for 4 hours
Good Vac = 5.0e-4 Torr
Bad Vac= 5.0 e-02 Torr
Initial IGP1= 4.07E-06 Torr
Thursday, June 08, 2023, 10:36
ramped @ 2A/min to 100A. Then after pressure stabilized starting ramp at 4A/min (2A/30s) to 400A
Thursday, June 08, 2023, 12:24
reached 1850 C with Set current = 480 and RD current = 470.6A, V = 7.7
Will leave for 4 hours.
Thursday, June 08, 2023, 15:31
ramping down at -2A/min (-1A/30s) |
Tuesday, June 06, 2023, 09:14, Darwin Ortiz Rosales, C, 44139-4, TARGET BOAT, Done, Graphite inside insert Experiment 2 (regular formulation discs)
|
Tuesday, June 06, 2023, 09:11
A Ta container tube was wrapped with 4 Ta heatshields. Note final container is 45220-6
272 graphite discs were loaded.
a TaC coated Ta spring at the front end.
The system was left to establish vacuum over previous night.
Good vacuum set to5e-04Torr
Bad vacuum was set to 5e-2 Torr
Total weight of system including spring= 253.94 g
OMEGA slope = 0.99
The target will be heated to ~2000 C, held there for 10 hours.
Initial ramp at 1A/min to 200A
Then ramp at 0.5A/min while taking temperature readings periodically unti l250A.
At 250 A will let pressure stabilize and then ramp at 1A/min to 2000C or 480A. Will use read back current
Will hold at target Temperature or Current for 10 hours before starting ramp-down.
Tuesday, June 06, 2023, 09:14
Starting ramt at 1A/min
initial IGP1= 8.2e-07
Tuesday, June 06, 2023, 21:25
@480 A on readback, 1823C on OMEGA. ramping to 510A set point which should be around 490 RD. (see heating profile for details)
Tuesday, June 06, 2023, 22:02
ramped to 516 on RD 527 on set. Will leave for 10 hours
OMEGA =1930 C
Wednesday, June 07, 2023, 06:32
OMEGA at 1950 C this morning. Will continue heating. Lowered to 1940 C as in experiment 1 this was the top temperature.
Wednesday, June 07, 2023, 07:40
OMEGA= 1940 C
IGP1=1.7-6 Torr
TGHT= 513A, 9.4V
starting ramp down at -2A/min |
Monday, June 05, 2023, 14:52, Aaron Schmidt, , , , , Swapped turbo pumps.
|
Previous TP would only spin up to 4KRPM. New TP installed.
Monday, June 05, 2023, 14:50: Roughing.
Monday, June 05, 2023, 15:10: Controller reset. TP on. |
Wednesday, May 24, 2023, 15:23, Darwin Ortiz Rosales, , 44139-4, LP TUBE, Done, Graphite inside insert Experiment 1
|
Wednesday, May 24, 2023, 15:22
A Ta container tube was wrapped with 4 Ta heatshields. Note final container is 45220-11
219 graphite discs were loaded.
a TaC coated Ta spring at the front end.
The system was left to establish vacuum over previous night.
Good vacuum set to5e-04Torr
Bad vacuum was set to 5e-2 Torr
Total weight of system including spring= 250.1 g
OMEGA slope = 0.99
The target will be heated to 2000 C, held there for 10 hours.
Initial ramp at 1A/min to 200A
Then ramp at 0.5A/min while taking temperature readings periodically unti l250A.
At 250 A will let pressure stabilize and then ramp at 1A/min to 2000C or 450A.
Will hold at target Temperature or Current for 10 hours before starting ramp-down.
Wednesday, May 24, 2023, 15:50
Currently heating at 0.5A/min to250A. Taking temperature/current measurements
IGP1= 1.06e-06 Torr
Wednesday, May 24, 2023, 18:28
heating at 1A/min to 275A to collect more temperature data
Wednesday, May 24, 2023, 19:22
Slight offset between set and RD current observed.
Ramping at 1A/min to 440A according to the regression below
Should be around 2000 C.
Wednesday, May 24, 2023, 20:22
Currently at 339 A, 4.8V
OMEGA = 1614 C, IGP1= 2.04e-06 Torr
Will ramp up at 2A/min to 450A as new data point suggests
Wednesday, May 24, 2023, 21:05
heating curve has new slope suggesting 500A as minimum to reach 2000 C
Increasing ramp to 1A/10s to reach 450A
Wednesday, May 24, 2023, 21:17
TGHT
IGP1= 3.9e-06 Torr
Continue ramping to 480A
Wednesday, May 24, 2023, 22:11
Offset between setpoint of current and readback. readback 10A below.
Will keep at this setting until 7:30 am tomorrow then start ramp down @-2A/min
Thursday, May 25, 2023, 07:25
OMEGA=1912C, IGP1 =1.29e-06 Torr, TGHT = 480A, 9.0V
begin ramp down at -2A/min
Thursday, May 25, 2023, 09:52
Some odd current readback behaeviour noticed. Have contacted Gelo from controls. He will look at it next week. Discrepancy between read back and set point and drop in read back currrent. See picture
|
Tuesday, May 02, 2023, 14:20, John Wong, np-TiO2, , TARGET BOAT, In progress, Carbonization of np-TiO2 spun fibrous pellets/fibre mats 7x
|
Tuesday, May 02, 2023, 14:03
Two np-TiO2 spun fibrous pellets and 1 batch of fibre mats were wrapped with graphite foils and loaded into a target boat.
Sample will be heated to 1875C, similar to the previous process, see e-log ID#605 (TGHT: 440A/7.6V).
TGHT will be autoramped to 350 A and monitor the conditions before ramping up further.
Good vacuum: 3e-5 Torr
Bad vacuum: 5e-5 Torr
Omega slope: 1.08
In the previous process (ID#605), Ta-foil was inserted at both ends of the tubes to hold the sample together. However, it was observed that the out-gassing of the material reacted with the Ta-foil, causing issues. Therefore, it's decided not to cover the ends with Ta-foil, and the sensor is now looking at the graphite foil. It had previously determined the slope for SiC material set for its emissivity, but need to note any errors that may have arisen due to the change in the sample setup.
See attachment#1 for sample setup - note that Omega sensor is slightly looking at the edge of the Ta-boat tube.
Initiate autoramp: 1 A/min
Chamber has been pumped down below 5.6e-6 Torr.
Tuesday, May 02, 2023, 15:31
Vacuum spike TGHT at 75A, auto-ramping down kicked in.
Wednesday, May 03, 2023, 12:18Thursday, May 04, 2023, 15:16
TGHT has been holding at 350A/5.7V (1995W) for almost 2hrs, temp is reading at 1368C - 232C lower than the previous process (ID#605) with TGHT = 348/5.8V (2018W).
Pressure started to come down around 344A/5.5V, temp 1331C - see attachment #2.
Current status overall view - see attachment #3
Continue to ramp up t0 440A at 1A/min and monitor.
Wednesday, May 03, 2023, 14:47
TGHT reached 440A/7.5V, temp reading at 1672C. Pressure is coming down, currently at 1.8e-6 Torr. Will keep at this setting overnight and will check the Omega/emmissivity to confirm the temperature.
Thursday, May 04, 2023, 10:54
Eractic vacuum spikes started just over 3 hrs ago. Temp at 1681 C; TGHT has been stable at 440A/7.6V. Pressure ranging between 5.0e-7 to 1.5 e-6 and gradually decreasing, see attachment #4.
Will perform the omega/emmissivity measurement.
Thursday, May 04, 2023, 15:16
Temperature was checked with the digital and analogue pyrometers.
With the analogue pyrometer on the Ta-container (left end, top surface), measured temp = 1360 C, with e=0.22, correction + 200 C => 1560 C
With the Omega pyrometer (right end), 1-color mode with e= 0.22, temp = 1585 C.
Setting Omega pyrometer to 2-color mode with e= 0.99 temp = 1516 C -- this is in agreement with the measurements for Ta. Note that the pyrometer is looking at some part of the Ta container which is not covered by the sample wrapped with the graphite foil (see attachment #5).
From e-log#596, temp was reported at 1520 C (slope at 0.99) with a Ta-foil at the end of the tube, but from e-log#605, temp was reported at 1864 C (slope at 0.99) - possibly an error occurred during that time.
In conclusion, the temp should be at 1530 C +/- 10C with TGHT = 440A/7.7V (3388W).
Thursday, May 04, 2023, 15:43
Vacuum spikes continue every 30 min lasting for 10 min.
Tapped down TGHT to 430A/7.5V, temp reading at 1500 C. Will monitor if any improvement with the vacuum.
Friday, May 05, 2023, 09:34
Vacuum spikes continue to happen; see attachment #6 for the striptool overview.
Lower TGHT to 420A/7.3V, temp = 1480 C.
Friday, May 05, 2023, 10:10
Vacuum spikes continue every 20-30 min lasting for 10 min.
Lower TGHT to 410A/7.1V, temp = 1450 C
Friday, May 05, 2023, 11:25
Vacuum spikes continue,
Lower TGHT to 400A/6.93V, temp = 1433 C
Friday, May 05, 2023, 12:20
Vacuum spikes - lower TGHT to 390A/6.7V, temp at 1407C
Friday, May 05, 2023, 13:19
Vacuum spikes - lower TGHT to 380A/6.5V, temp at 1388C
Friday, May 05, 2023, 13:47
Vacuum spikes - lower TGHT to 370A/6.3V, temp at1373 C
Friday, May 05, 2023, 14:16
Vacuum spikes - lower TGHT 360A/6.1V, temp at 1348 C
Friday, May 05, 2023, 15:11
Vacuum spikes - lower TGHT 350A/5.9V, temp at 1308 C
Friday, May 05, 2023, 16:34
Vacuum spikes - lower TGHT 340A/5.7V, temp at 1371 C
Friday, May 05, 2023, 16:56
Vacuum spikes continue; container possibly broken.
Slow ramp down TGHT at -0.5A/min to see when the vacuum spikes would stop.
Monday, May 08, 2023, 09:54
TGHT was ramped down over the weekend. Chamber was kept under vacuum and vacuum continued to spike; suspecting problem with the gauge?! see attachment &7 for an over view.
Will take out the samples for exam.
|
Friday, April 28, 2023, 11:31, Darwin Ortiz Rosales, TaC, Boat, TARGET BOAT, Done, TaC coated endcaps and spring sintering
|
Friday, April 28, 2023, 11:29
loaded 14 TaC coated end caps and 2 TaC coated springs.
OMEGA Slope 0.99
Will heat to 1850-1900 C and hold for 4 hours
Good Vac = 5.0e-4 Torr
Bad Vac= 5.0 e-02 Torr
2 end caps had slight damage and were disposed of. 12 good caps and 2 good springs. |
Wednesday, April 26, 2023, 09:48, Darwin Ortiz Rosales, TiC, 44692-5, LP-FEBIAD, Done, TiC230425
|
Wednesday, April 26, 2023, 09:32
LP FEBIAD loaded with 367 TiC discs and 4 TiC removable discs for analyses
50 packs of 5 and the rest are singles
TaC coated (sintered) springs placed at both ends
Initial total Weight = 521.83 g
Initial heating @ 1A/min to 400 A on TGHT and 280A on TBHT
OMEGA slope = 0.99
Vacuum limits up to 200A: 3.0e-05 Torr -- 5.0e-04 Torr
Vacuum limit up after 200A: 3.0e-05 Torr -- 5.0e-05 Torr
No Ta heat-shields used
Initial IGP1 = 4.1e-07 Torr
Wednesday, April 26, 2023, 09:49
Starting initial ramp up to 200A on both TGHT and TBHT @ 1A/min
Wednesday, April 26, 2023, 12:50
Around 120A on TGHT, the pressure started to slowly drop. First outgassing done.
Wednesday, April 26, 2023, 14:03
IGP1 = 6.0 e-05 Torr
TGHT = 200 A, 2.7V
TBHT = 200 A, 2.6 v
OMEGA = Below lower limit
Waiting for pressure to fall below 5e0-5 Torr. Will change bad vacuum to 5.0e-05 Torr and then continue ramping @1A/min to 400 A on TGHT and 280 A on TBHT.
Wednesday, April 26, 2023, 14:13
IGPI= 4.2 e-05 Torr
starting ramping to 400 A on TGHT and 280A on TBHT
Wednesday, April 26, 2023, 14:26
The IGP1 pressure just fell below 3.0e-05 Torr and ramping has resumed
Wednesday, April 26, 2023, 14:42
pressure hovering around good vacuum so very slow progress.
Wednesday, April 26, 2023, 15:12
TGHT= 223 A, 3.1 V
TBHT = 226 A, 3.0 V
Set ramp rate is 1A/min but real rate is slightly less than 0.5A/min due to pressure fluctuation. |
Wednesday, April 26, 2023, 18:20, Carla Babcock, TiC, 44692-5, LP-FEBIAD, In progress, TiC230425
|
Darwin Ortiz Rosales wrote: |
Wednesday, April 26, 2023, 09:32
LP FEBIAD loaded with 367 TiC discs and 4 TiC removable discs for analyses
50 packs of 5 and the rest are singles
TaC coated (sintered) springs placed at both ends
Initial total Weight = 521.83 g
Initial heating @ 1A/min to 400 A on TGHT and 280A on TBHT
OMEGA slope = 0.99
Vacuum limits up to 200A: 3.0e-05 Torr -- 5.0e-04 Torr
Vacuum limit up after 200A: 3.0e-05 Torr -- 5.5e-05 Torr
No Ta heat-shields used
Initial IGP1 = 4.1e-07 Torr
Wednesday, April 26, 2023, 09:49
Starting initial ramp up to 200A on both TGHT and TBHT @ 1A/min
Wednesday, April 26, 2023, 12:50
Around 120A on TGHT, the pressure started to slowly drop. First outgassing done.
Wednesday, April 26, 2023, 14:03
IGP1 = 6.0 e-05 Torr
TGHT = 200 A, 2.7V
TBHT = 200 A, 2.6 v
OMEGA = Below lower limit
Waiting for pressure to fall below 5e0-5 Torr. Will change bad vacuum to 5.0e-05 Torr and then continue ramping @1A/min to 400 A on TGHT and 280 A on TBHT.
Wednesday, April 26, 2023, 14:13
IGPI= 4.2 e-05 Torr
starting ramping to 400 A on TGHT and 280A on TBHT
Wednesday, April 26, 2023, 14:26
The IGP1 pressure just fell below 3.0e-05 Torr and ramping has resumed
Wednesday, April 26, 2023, 14:42
pressure hovering around good vacuum so very slow progress.
Wednesday, April 26, 2023, 15:12
TGHT= 223 A, 3.1 V
TBHT = 226 A, 3.0 V
Set ramp rate is 1A/min but real rate is slightly less than 0.5A/min due to pressure fluctuation.
|
Vacuum spike at 300A.
Currently:
TGHT= 316A, 4.6V
TBHT=283A, 3.9V
Wednesday, April 26, 2023, 18:18 Ramping TBHT down from 280A to 270A |
Wednesday, April 26, 2023, 22:26, John Wong, TiC, 44692-5, LP-FEBIAD, In progress, TiC230425
|
Carla Babcock wrote: |
Darwin Ortiz Rosales wrote: |
Wednesday, April 26, 2023, 09:32
LP FEBIAD loaded with 367 TiC discs and 4 TiC removable discs for analyses
50 packs of 5 and the rest are singles
TaC coated (sintered) springs placed at both ends
Initial total Weight = 521.83 g
Initial heating @ 1A/min to 400 A on TGHT and 280A on TBHT
OMEGA slope = 0.99
Vacuum limits up to 200A: 3.0e-05 Torr -- 5.0e-04 Torr
Vacuum limit up after 200A: 3.0e-05 Torr -- 5.5e-05 Torr
No Ta heat-shields used
Initial IGP1 = 4.1e-07 Torr
Wednesday, April 26, 2023, 09:49
Starting initial ramp up to 200A on both TGHT and TBHT @ 1A/min
Wednesday, April 26, 2023, 12:50
Around 120A on TGHT, the pressure started to slowly drop. First outgassing done.
Wednesday, April 26, 2023, 14:03
IGP1 = 6.0 e-05 Torr
TGHT = 200 A, 2.7V
TBHT = 200 A, 2.6 v
OMEGA = Below lower limit
Waiting for pressure to fall below 5e0-5 Torr. Will change bad vacuum to 5.0e-05 Torr and then continue ramping @1A/min to 400 A on TGHT and 280 A on TBHT.
Wednesday, April 26, 2023, 14:13
IGPI= 4.2 e-05 Torr
starting ramping to 400 A on TGHT and 280A on TBHT
Wednesday, April 26, 2023, 14:26
The IGP1 pressure just fell below 3.0e-05 Torr and ramping has resumed
Wednesday, April 26, 2023, 14:42
pressure hovering around good vacuum so very slow progress.
Wednesday, April 26, 2023, 15:12
TGHT= 223 A, 3.1 V
TBHT = 226 A, 3.0 V
Set ramp rate is 1A/min but real rate is slightly less than 0.5A/min due to pressure fluctuation.
|
Vacuum spike at 300A.
Currently:
TGHT= 316A, 4.6V
TBHT=283A, 3.9V
Wednesday, April 26, 2023, 18:18 Ramping TBHT down from 280A to 270A
|
Wednesday, April 26, 2023, 22:12
TGHT = 400A, 6.1V; TBHT = 274A/3.7V. Temp is holding sturdy ~1100 C and will leave it overnight.
Pressure is coming down, currently at 8.8 e-6 Torr. See attachment for the overview.
TGHT will continue to ramp up tomorrow morning; check the pressure to ensure it has come down below 5e-6 Torr before proceeding. Refer to the instructions for details.
|
Thursday, April 27, 2023, 06:30, Darwin Ortiz Rosales, TiC, 44692-5, LP-FEBIAD, Done, TiC230425
|
John Wong wrote: |
Carla Babcock wrote: |
Darwin Ortiz Rosales wrote: |
Wednesday, April 26, 2023, 09:32
LP FEBIAD loaded with 367 TiC discs and 4 TiC removable discs for analyses
50 packs of 5 and the rest are singles
TaC coated (sintered) springs placed at both ends
Initial total Weight = 521.83 g
Initial heating @ 1A/min to 400 A on TGHT and 280A on TBHT
OMEGA slope = 0.99
Vacuum limits up to 200A: 3.0e-05 Torr -- 5.0e-04 Torr
Vacuum limit up after 200A: 3.0e-05 Torr -- 5.5e-05 Torr
No Ta heat-shields used
Initial IGP1 = 4.1e-07 Torr
Wednesday, April 26, 2023, 09:49
Starting initial ramp up to 200A on both TGHT and TBHT @ 1A/min
Wednesday, April 26, 2023, 12:50
Around 120A on TGHT, the pressure started to slowly drop. First outgassing done.
Wednesday, April 26, 2023, 14:03
IGP1 = 6.0 e-05 Torr
TGHT = 200 A, 2.7V
TBHT = 200 A, 2.6 v
OMEGA = Below lower limit
Waiting for pressure to fall below 5e0-5 Torr. Will change bad vacuum to 5.0e-05 Torr and then continue ramping @1A/min to 400 A on TGHT and 280 A on TBHT.
Wednesday, April 26, 2023, 14:13
IGPI= 4.2 e-05 Torr
starting ramping to 400 A on TGHT and 280A on TBHT
Wednesday, April 26, 2023, 14:26
The IGP1 pressure just fell below 3.0e-05 Torr and ramping has resumed
Wednesday, April 26, 2023, 14:42
pressure hovering around good vacuum so very slow progress.
Wednesday, April 26, 2023, 15:12
TGHT= 223 A, 3.1 V
TBHT = 226 A, 3.0 V
Set ramp rate is 1A/min but real rate is slightly less than 0.5A/min due to pressure fluctuation.
|
Vacuum spike at 300A.
Currently:
TGHT= 316A, 4.6V
TBHT=283A, 3.9V
Wednesday, April 26, 2023, 18:18 Ramping TBHT down from 280A to 270A
|
Wednesday, April 26, 2023, 22:12
TGHT = 400A, 6.1V; TBHT = 274A/3.7V. Temp is holding sturdy ~1100 C and will leave it overnight.
Pressure is coming down, currently at 8.8 e-6 Torr. See attachment for the overview.
TGHT will continue to ramp up tomorrow morning; check the pressure to ensure it has come down below 5e-6 Torr before proceeding. Refer to the instructions for details.
|
Thursday, April 27, 2023, 06:27
IGP1= 1.7e-06 Torr
OMEGA= 1097 C
TGHT= 400A, 6.2V
TBHT= 273A, 3.7 V
Starting ramp up of TGHT @0.2A/min set to 550A |
Thursday, April 27, 2023, 21:48, Carla Babcock, TiC, 44692-5, LP-FEBIAD, In progress, TiC230425
|
Darwin Ortiz Rosales wrote: |
John Wong wrote: |
Carla Babcock wrote: |
Darwin Ortiz Rosales wrote: |
Wednesday, April 26, 2023, 09:32
LP FEBIAD loaded with 367 TiC discs and 4 TiC removable discs for analyses
50 packs of 5 and the rest are singles
TaC coated (sintered) springs placed at both ends
Initial total Weight = 521.83 g
Initial heating @ 1A/min to 400 A on TGHT and 280A on TBHT
OMEGA slope = 0.99
Vacuum limits up to 200A: 3.0e-05 Torr -- 5.0e-04 Torr
Vacuum limit up after 200A: 3.0e-05 Torr -- 5.5e-05 Torr
No Ta heat-shields used
Initial IGP1 = 4.1e-07 Torr
Wednesday, April 26, 2023, 09:49
Starting initial ramp up to 200A on both TGHT and TBHT @ 1A/min
Wednesday, April 26, 2023, 12:50
Around 120A on TGHT, the pressure started to slowly drop. First outgassing done.
Wednesday, April 26, 2023, 14:03
IGP1 = 6.0 e-05 Torr
TGHT = 200 A, 2.7V
TBHT = 200 A, 2.6 v
OMEGA = Below lower limit
Waiting for pressure to fall below 5e0-5 Torr. Will change bad vacuum to 5.0e-05 Torr and then continue ramping @1A/min to 400 A on TGHT and 280 A on TBHT.
Wednesday, April 26, 2023, 14:13
IGPI= 4.2 e-05 Torr
starting ramping to 400 A on TGHT and 280A on TBHT
Wednesday, April 26, 2023, 14:26
The IGP1 pressure just fell below 3.0e-05 Torr and ramping has resumed
Wednesday, April 26, 2023, 14:42
pressure hovering around good vacuum so very slow progress.
Wednesday, April 26, 2023, 15:12
TGHT= 223 A, 3.1 V
TBHT = 226 A, 3.0 V
Set ramp rate is 1A/min but real rate is slightly less than 0.5A/min due to pressure fluctuation.
|
Vacuum spike at 300A.
Currently:
TGHT= 316A, 4.6V
TBHT=283A, 3.9V
Wednesday, April 26, 2023, 18:18 Ramping TBHT down from 280A to 270A
|
Wednesday, April 26, 2023, 22:12
TGHT = 400A, 6.1V; TBHT = 274A/3.7V. Temp is holding sturdy ~1100 C and will leave it overnight.
Pressure is coming down, currently at 8.8 e-6 Torr. See attachment for the overview.
TGHT will continue to ramp up tomorrow morning; check the pressure to ensure it has come down below 5e-6 Torr before proceeding. Refer to the instructions for details.
|
Thursday, April 27, 2023, 06:27
IGP1= 1.7e-06 Torr
OMEGA= 1097 C
TGHT= 400A, 6.2V
TBHT= 273A, 3.7 V
Starting ramp up of TGHT @0.2A/min set to 550A
|
Reached 550A on TGHT (paused there until I realized it was stopped) then resumed ramping to 580A at 0.2A/min. Saw both vacuum spikes before 550A. Attaching screenshot from John. |
Thursday, April 27, 2023, 22:18, John Wong, TiC, 44692-5, LP-FEBIAD, In progress, TiC230425
|
Darwin Ortiz Rosales wrote: |
John Wong wrote: |
Carla Babcock wrote: |
Darwin Ortiz Rosales wrote: |
Wednesday, April 26, 2023, 09:32
LP FEBIAD loaded with 367 TiC discs and 4 TiC removable discs for analyses
50 packs of 5 and the rest are singles
TaC coated (sintered) springs placed at both ends
Initial total Weight = 521.83 g
Initial heating @ 1A/min to 400 A on TGHT and 280A on TBHT
OMEGA slope = 0.99
Vacuum limits up to 200A: 3.0e-05 Torr -- 5.0e-04 Torr
Vacuum limit up after 200A: 3.0e-05 Torr -- 5.5e-05 Torr
No Ta heat-shields used
Initial IGP1 = 4.1e-07 Torr
Wednesday, April 26, 2023, 09:49
Starting initial ramp up to 200A on both TGHT and TBHT @ 1A/min
Wednesday, April 26, 2023, 12:50
Around 120A on TGHT, the pressure started to slowly drop. First outgassing done.
Wednesday, April 26, 2023, 14:03
IGP1 = 6.0 e-05 Torr
TGHT = 200 A, 2.7V
TBHT = 200 A, 2.6 v
OMEGA = Below lower limit
Waiting for pressure to fall below 5e0-5 Torr. Will change bad vacuum to 5.0e-05 Torr and then continue ramping @1A/min to 400 A on TGHT and 280 A on TBHT.
Wednesday, April 26, 2023, 14:13
IGPI= 4.2 e-05 Torr
starting ramping to 400 A on TGHT and 280A on TBHT
Wednesday, April 26, 2023, 14:26
The IGP1 pressure just fell below 3.0e-05 Torr and ramping has resumed
Wednesday, April 26, 2023, 14:42
pressure hovering around good vacuum so very slow progress.
Wednesday, April 26, 2023, 15:12
TGHT= 223 A, 3.1 V
TBHT = 226 A, 3.0 V
Set ramp rate is 1A/min but real rate is slightly less than 0.5A/min due to pressure fluctuation.
|
Vacuum spike at 300A.
Currently:
TGHT= 316A, 4.6V
TBHT=283A, 3.9V
Wednesday, April 26, 2023, 18:18 Ramping TBHT down from 280A to 270A
|
Wednesday, April 26, 2023, 22:12
TGHT = 400A, 6.1V; TBHT = 274A/3.7V. Temp is holding sturdy ~1100 C and will leave it overnight.
Pressure is coming down, currently at 8.8 e-6 Torr. See attachment for the overview.
TGHT will continue to ramp up tomorrow morning; check the pressure to ensure it has come down below 5e-6 Torr before proceeding. Refer to the instructions for details.
|
Thursday, April 27, 2023, 06:27
IGP1= 1.7e-06 Torr
OMEGA= 1097 C
TGHT= 400A, 6.2V
TBHT= 273A, 3.7 V
Starting ramp up of TGHT @0.2A/min set to 550A
|
Thursday, April 27, 2023, 22:04
TGHT has reached 580A/10.33V. Temp = 1540C.
The two out-gassing peaks were observed: 1st peak around 1300C and 2nd peak 1370C. See attachments 1 & 2.
A few minutes after TGHT reached to 580A, there was a small jump in TGHT current/voltage and also the pressure, but didn't notice any change in the temp, see attachment 3&4.
Pressure is currently at 3.4e-6 Torr; will hold TGHT until pressure reaches close to 1e-6 Torr before cooling down.
Friday, April 28, 2023, 01:06
Pressure has reached 1.8 e-6 Torr; TGHT has been holding at 580A for 3.5 hrs, a slight increase in voltage, reading at 10.45V and temperature, 1548C. See attachment #5 for overview.
Initiating auto-cooling TGHT at -2A/min, TBHT at -1A/min.
|
Friday, April 28, 2023, 09:39, Darwin Ortiz Rosales, TiC, 44692-5, LP-FEBIAD, Done, TiC230425
|
John Wong wrote: |
Darwin Ortiz Rosales wrote: |
John Wong wrote: |
Carla Babcock wrote: |
Darwin Ortiz Rosales wrote: |
Wednesday, April 26, 2023, 09:32
LP FEBIAD loaded with 367 TiC discs and 4 TiC removable discs for analyses
50 packs of 5 and the rest are singles
TaC coated (sintered) springs placed at both ends
Initial total Weight = 521.83 g
Initial heating @ 1A/min to 400 A on TGHT and 280A on TBHT
OMEGA slope = 0.99
Vacuum limits up to 200A: 3.0e-05 Torr -- 5.0e-04 Torr
Vacuum limit up after 200A: 3.0e-05 Torr -- 5.5e-05 Torr
No Ta heat-shields used
Initial IGP1 = 4.1e-07 Torr
Wednesday, April 26, 2023, 09:49
Starting initial ramp up to 200A on both TGHT and TBHT @ 1A/min
Wednesday, April 26, 2023, 12:50
Around 120A on TGHT, the pressure started to slowly drop. First outgassing done.
Wednesday, April 26, 2023, 14:03
IGP1 = 6.0 e-05 Torr
TGHT = 200 A, 2.7V
TBHT = 200 A, 2.6 v
OMEGA = Below lower limit
Waiting for pressure to fall below 5e0-5 Torr. Will change bad vacuum to 5.0e-05 Torr and then continue ramping @1A/min to 400 A on TGHT and 280 A on TBHT.
Wednesday, April 26, 2023, 14:13
IGPI= 4.2 e-05 Torr
starting ramping to 400 A on TGHT and 280A on TBHT
Wednesday, April 26, 2023, 14:26
The IGP1 pressure just fell below 3.0e-05 Torr and ramping has resumed
Wednesday, April 26, 2023, 14:42
pressure hovering around good vacuum so very slow progress.
Wednesday, April 26, 2023, 15:12
TGHT= 223 A, 3.1 V
TBHT = 226 A, 3.0 V
Set ramp rate is 1A/min but real rate is slightly less than 0.5A/min due to pressure fluctuation.
|
Vacuum spike at 300A.
Currently:
TGHT= 316A, 4.6V
TBHT=283A, 3.9V
Wednesday, April 26, 2023, 18:18 Ramping TBHT down from 280A to 270A
|
Wednesday, April 26, 2023, 22:12
TGHT = 400A, 6.1V; TBHT = 274A/3.7V. Temp is holding sturdy ~1100 C and will leave it overnight.
Pressure is coming down, currently at 8.8 e-6 Torr. See attachment for the overview.
TGHT will continue to ramp up tomorrow morning; check the pressure to ensure it has come down below 5e-6 Torr before proceeding. Refer to the instructions for details.
|
Thursday, April 27, 2023, 06:27
IGP1= 1.7e-06 Torr
OMEGA= 1097 C
TGHT= 400A, 6.2V
TBHT= 273A, 3.7 V
Starting ramp up of TGHT @0.2A/min set to 550A
|
Thursday, April 27, 2023, 22:04
TGHT has reached 580A/10.33V. Temp = 1540C.
The two out-gassing peaks were observed: 1st peak around 1300C and 2nd peak 1370C. See attachments 1 & 2.
A few minutes after TGHT reached to 580A, there was a small jump in TGHT current/voltage and also the pressure, but didn't notice any change in the temp, see attachment 3&4.
Pressure is currently at 3.4e-6 Torr; will hold TGHT until pressure reaches close to 1e-6 Torr before cooling down.
Friday, April 28, 2023, 01:06
Pressure has reached 1.8 e-6 Torr; TGHT has been holding at 580A for 3.5 hrs, a slight increase in voltage, reading at 10.45V and temperature, 1548C. See attachment #5 for overview.
Initiating auto-cooling TGHT at -2A/min, TBHT at -1A/min.
|
Friday, April 28, 2023, 09:27
IGP1= 1.20e-07 Torr
Will dismount target around 10:15 am
Heating curve below. Non-linear behavior
Final weight = 517.08 g
Target looks good see attached picture
|
Monday, April 24, 2023, 09:12, Darwin Ortiz Rosales, TaC, 44692-5, LP-FEBIAD, Done, TaC coating sintering
|
Sunday, April 23, 2023, 07:23
The coated container was wrapped in 3 Ta foil heatshields.
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230A
Final TGHT current= ~450A (adjustable)
Good vacuum = 5.0 e-04Torr
Bad vacuum = 5.0E-02 Torr
Interlock tripped (HS water flow, SP6, GE, CHIL <--supposed to be bypassed)
Monday, April 24, 2023, 13:24
In the morning Carla found some loose wires behind EVAP 2. Wires connecting the flow-meter. The interlock problem was fixed as it was noted there was normal HS water flow.
Started ramp up at 1A/min to 230 A. The first outgassing bump observed and wil start autoramp @ 2A/min on both TGHT and TBHT (target is 400A on TGHT and 230A on TBHT).
Monday, April 24, 2023, 16:24
Reached 480A on TGHT at 4 pm. Manually tapped to 500 A on TGHT , OMEGA=1853C. Will keep until 8 pm.
Monday, April 24, 2023, 19:56
OMEGA= 1853 C
IGP1= 1.5e-06 Torr
TGHT = 500A, 8.5V
TBHT= 230A, 3.1V
rampdown TGHT @-2A/min and TBHT @ -1A/min
|
Thursday, April 20, 2023, 07:00, Darwin Ortiz Rosales, TaC, 41790-7, LP-FEBIAD, Done, TaC coating sintering
|
Thursday, April 20, 2023, 06:59
The coated container was wrapped in 3 Ta foil heatshields.
Target temperature on OMEGA= 1830-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230A
Final TGHT current= ~400A (adjustable)
Good vacuum = 5.0 e-04 Torr
Bad vacuum = 5.0E-02 Torr
Thursday, April 20, 2023, 07:02
Started TBHT and TBHT ramp at 1A/min to 230A
Thursday, April 20, 2023, 09:55
From 170 A started ramping at 2A/min to 230 A on both TGHT and TBHT
Thursday, April 20, 2023, 10:27
Starting ramp on TGHT to 300A, TBHT kept at 230A, 3.0 V
Thursday, April 20, 2023, 11:19
ramping at 4A/min (2A/30s) to 340 A on TGHT
Thursday, April 20, 2023, 11:40
After plot, ramping @ 2A/min to 460A on TGHT expected to reeach at 1245. 4 hours at 4:45 pm
Thursday, April 20, 2023, 13:44
Note that top temperature was 1835C @ 480 A, 7.9V
Thursday, April 20, 2023, 17:00
Start rampdown at -2A/min TGHT and -1A/min TBHT
Monday, April 24, 2023, 13:35
The coating is not as good as expected. Maybe too much time between coating and sintering. Will not use for TiC target. |
Tuesday, April 18, 2023, 06:48, Darwin Ortiz Rosales, TaC, 45220-11, LP-SIS, Done, TaC coating sintering
|
Tuesday, April 18, 2023, 06:46
The coated container was wrapped in four Ta foil heatshields.
Target temperature on OMEGA= 1830-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230A
Final TGHT current= ~400A (adjustable)
Good vacuum = 5.0 e-04 Torr
Bad vacuum = 5.0E-02Torr
Tuesday, April 18, 2023, 06:47
IGP1 initial = 3.80e-07 Torr
Start ramp up at 2A min to 230 on both TBHT and TGHT
Tuesday, April 18, 2023, 09:43
Autoramping TGHT to 380 A @4/min (2/A 30s)
Tuesday, April 18, 2023, 10:36
manually ramped to 416A, 6.8 V on TGHT
TBHT = 230 A, 4.0V
Holding here for 4 hours.
OMEGA = 1863 c
Tuesday, April 18, 2023, 11:26
increased current on TGHT to 418 because temperature had slipped below 1850 C
Tuesday, April 18, 2023, 14:52
ramping down @-2A/min TGHT and -1A/min TBHT |
Sunday, April 16, 2023, 14:08, Darwin Ortiz Rosales, TaC, 45220-14, LP-SIS, Done, TaC coating sintering
|
Sunday, April 16, 2023, 14:08
The coated container was wrapped in four Ta foil heatshields.
Target temperature on OMEGA= 1860-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230A
Final TGHT current= ~400A (adjustable)
Good vacuum = 5.0 e-04 Torr
Bad vacuum = 5.0E-02 Torr
Ramped at 2A/min to 230 A on both TGHT and TBHT.
Then ramped @4A/min to 385 A on TGHT. Then ramped manually to 1850 C
Sunday, April 16, 2023, 18:31
At 428A reached 1830C on OMEGA
Sunday, April 16, 2023, 22:24
Start ramp down @ -2A/min TGHT and -1A/min TBHT |
Wednesday, April 12, 2023, 09:53, Darwin Ortiz Rosales, TaC, , TARGET BOAT, Done, TaC coating sintering
|
Wednesday, April 12, 2023, 09:53
The coated container was wrapped in 3 Ta foil heatshields.
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= N/A
Final TGHT current= ~400A (adjustable)
Heating autoramp starged at 4A/min on TGHT 40A
Then at 2A/min to 90 A.
Good vacuum = 5.0 e-04 Torr
Bad vacuum = 5.0E-02 Torr
IGP1 initial = 4.7e-07 Torr
Wednesday, April 12, 2023, 10:46
heating at 2A/min to 90A
Wednesday, April 12, 2023, 11:18
Autoramping at 2A/min to 230A
Wednesday, April 12, 2023, 11:53
Autoramping at 4A/min to 230 A
Wednesday, April 12, 2023, 13:57
Autoramping to 380A
Wednesday, April 12, 2023, 14:07
manually adjusted TGHT to 384A. 6.6 V
OMEGA reads 1859 C. Leaving for 4 hours.
Wednesday, April 12, 2023, 18:36
Started rampdown at -2A/min |
Tuesday, April 04, 2023, 12:50, Darwin Ortiz Rosales, TaC, 45447-1, HP-FEBIAD, Done, TaC coating sintering
|
Tuesday, April 04, 2023, 12:48
Ta HP-FEBIAD was coated with TaC and wrapped with Ta heat-shields (3 layers + 1 inner layer around fins including center fins)
Desired temperature = 1850 C , TBHT will be set fixed at 230A (max).
Evap 2 will be pumped down over previous night
OMEGA slope= 0.990
Good vacuum = 5.00 e-4 Torr
Bad vacuum = 5.00 e-2 Torr
OMEGA target temp = 1850 C
Wednesday, April 05, 2023, 07:37
IGP1= 4.3e-07 Torr
starting autoramp @ 1A/min to 230A on both TGHT and TBHT
Wednesday, April 05, 2023, 10:56
Starting Autoramp at 4A/min to 400 A on TGHT
Wednesday, April 05, 2023, 14:14
OMEGA Reached 1877C @ 743A, 11.3V TGHT
rampdown @ 6:00 pm
Wednesday, April 05, 2023, 14:38
Decreased TGHT current to 736A because temperature was creeping up
rampdown was started at 6:05 pm
Final pressure at 0 V - 1.7e-07 Torr
|
Thursday, March 30, 2023, 12:45, Aaron Schmidt, Ta, 45220-7, LP-SIS, In progress, Conditioning Ta#65
|
Thursday, March 30, 2023, 12:27:
Ta#65 LP-SIS target description:
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.033mm (0.0013") avg Measured.
Target material batch: Ta 2023-1 Mt'l PO# TR-2022-03028
Target density = 18.2685 g/cm3
Target length = 3.40 cm
Total Mass = 62.113 g [Incl foils + Ta wire on 6 packs]
Total mass w/ Target oven= 460.8 g (w/ end caps)
Discs in target are arranged as follows: 1pack / 75 singles / 1pack / 100 singles / 2packs / 100 singles / 1pack / 75 singles / 1pack
Dimpling direction on foils/ Packs. --> Center <--
End caps installed (Not expanded). No Ta foil heat shield added
Tuesday, May 16, 2023, 10:44: End cap removed post conditioning to remove the rhenium foil. End cap replaced, & weight updated. Length remains the same.
Final desired temperature = 1900C.
Thursday, March 30, 2023, 12:41: RP on.
Thursday, March 30, 2023, 12:42: Roughing
Thursday, March 30, 2023, 12:44: OMEGA slope = 0.98.
Thursday, March 30, 2023, 12:59: TP1 on.
Thursday, March 30, 2023, 13:00: TP1 off.
Thursday, March 30, 2023, 13:03: Venting. (Steel pair of shields req'd - Install)
Thursday, March 30, 2023, 13:05: Roughing.
Thursday, March 30, 2023, 13:20: TP1 on.
Thursday, March 30, 2023, 13:29: TP1 trip @ 38 krpm. Quick Reset. Fully "green". OK.
Thursday, March 30, 2023, 13:31: Vacuum @ 5.84e-05T. TGHT / TBHT PS on.
Thursday, March 30, 2023, 13:32: Operation Check. TGHT / TBHT tapped up to 5 / 5 A. Ok. Back to 0A.
Friday, March 31, 2023, 06:32: Auto-ramping TGHT / TBHT to 500 / 200 A @ 2 A per minute. Vacuum @ 6.52e-07T.
Friday, March 31, 2023, 12:08: TGHT / TBHT @ 500 / 200 A. Vacuum @ 2.24e-06T. Temperature @ 1575 C. Auto-ramping TGHT / TBHT to 580 / 230 A @ 2 A per min
Friday, March 31, 2023, 13:05: TGHT / TBHT @ 580 / 230 A. Vacuum @ 3.69e-06T. Temperature @ 1748 C. Auto-ramping TGHT to 600 @ 2 A per min
Friday, March 31, 2023, 13:27: TGHT / TBHT @ 600 / 230 A. Vacuum @ 3.83e-06T. Temperature @ 1790 C. Auto-ramping TGHT to 620 @ 2 A per min
Friday, March 31, 2023, 13:42: TGHT / TBHT @ 620 / 230 A. Vacuum @ 4.34e-06T. Temperature @ 1820 C. Auto-ramping TGHT to 640 @ 2 A per min
Friday, March 31, 2023, 13:51: TGHT / TBHT @ 640 / 230 A. Vacuum @ 5.51e-06T. Temperature @ 1858 C. Tap up TGHT to 650 A
Friday, March 31, 2023, 13:54: Vacuum @ 6.03e-06T. Temp @ 1902 C. Tapped up TGHT to 660 manually. Desired temperature reached.
Friday, March 31, 2023, 13:57: Auto-cooling @ 2 A per minute.
Friday, March 31, 2023, 17:31:
Monday, April 03, 2023, 07:35: PS off. TP off. |
Thursday, March 16, 2023, 14:47, Darwin Ortiz Rosales, TaC, 45220-9, LP-SIS, Done, TaC coating sintering
|
Thursday, March 16, 2023, 13:38
The coated container was wrapped in four Ta foil heatshields.
Target temperature on OMEGA= 1860-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230A
Final TGHT current= ~400A (adjustable)
Good vacuum = 5.0 e-02 Torr
Bad vacuum = 5.0E-04 Torr
Thursday, March 16, 2023, 22:21
Started ramping TGHT and TBHT @ 1.5A/min to 387 A and 230A respectively.
IGP1 initial = 9.6 e-07 Torr
Cooling projected at 6:48 am tomorrow.
Friday, March 17, 2023, 06:59
Final IGP1= 1.6e-o6 Torr
Started rampdown @-2A/min TGHT and -1A/min TBHT
Coating looks good uniformely.
OMEGA 1850 C (was 1868 initially)
TGHT was 387A, 6.6 V and TBHT was 230A, 4.1 V
Coating very nice |
Monday, March 13, 2023, 22:31, Darwin Ortiz Rosales, SiC, 44692-2, HP-SIS, Done, SiC-230313
|
Monday, March 13, 2023, 22:28
Total number of foils:380 ( including 5 analysis discs on the front side of the container)
Total length packed 17 cm (excluding 5 analysis discs that will be removed)
container has 4 Ta heat shields (one inner only around fins)
No endcaps inserted to facilitate out-gassing
Ta coated spring at both ends
ramp to 500A @ 1A/min TGHT and to 230A on TBHT
max approx 700A on TGHT and 230A on TBHT (Omega slope set = 0.990)
Then temperature = 1800 C. Will ramp to 1820 C
TBHT will be set fixed at 230 A (max). TBHT heated manually and automatically to max.
Good vac at 5.00 e -4 Torr
Bad vac at 5.00 e-2 Torr
IGP1= 2.8e-06 Torr at start of initial ramp.
Tuesday, March 14, 2023, 07:26
Increased autoramp to 2A/min to 700 A on TGHT while keeping TBHT to 230A, 3.3V
Tuesday, March 14, 2023, 09:53
At 743A, 11.8V TGHT
OMEGA = 1780 C. (not entirely reliable, will leave at this current for 4 hours)
Tuesday, March 14, 2023, 14:00
Starting rampdown at -2A/min on TGHT and -1A/min TBHT
Final IGP1= 5.5e-06 Torr
OMEGA= 1750C
TBHT= 230A, 3.3V
|
Sunday, March 12, 2023, 08:06, Darwin Ortiz Rosales, Ta, 44692-2, HP-SIS, Done, TaC coating sintering
|
Sunday, March 12, 2023, 08:04
Ta HP-SIS was coated with TaC and wrapped with Ta heat-shields (3 layers + 1 inner layer around fins)
Desired temperature = 1850 C , TBHT will be set fixed at 230A (max).
Evap 2 will be pumped down over previous night
OMEGA slope= 0.990
Good vacuum = 5.00 e-4 Torr
Bad vacuum = 5.00 e-2 Torr
IGP1=1.9 e-07 Torr
Start autoramp @2A/min to120 A on TGHT and TBHT.
OMEGA target temp = 1850 C
Sunday, March 12, 2023, 13:08
start autoramp to 500A on TGHT @ 4A/min (2A/30s)
from 320A, 4.5 V on TGHT
IGP1= 6.8e-07 Torr
Sunday, March 12, 2023, 19:09
Starting ramp down @ -2A/min TGHT, and -1A/min TBHT
@687A, 10.7 V TGHT OMEGA = 1850 C
final pressure IGP1= 2.4e-06 Torr
|
Thursday, March 09, 2023, 06:58, Darwin Ortiz Rosales, Endcaps, , TARGET BOAT, Done, TaC coated endcaps and spring sintering
|
Thursday, March 09, 2023, 06:53
2 TaC coated springs and 12 Tac coated caps loaded into a target boat (in packs of 4 wrapped in graphite foil).
Target boat wrapped in 4 Ta heatshields
Target boat type was with endcaps at both ends.
Left in Evap2 over previous night to depressurize.
Target temperature= 1850-1900C for 4 hours
Good vacuum = 5e-04 Torr
Bad vacuum = 5e-02 Torr
Start autoramp at 2A/min to 50A on TGHT
Thursday, March 09, 2023, 07:22
at 44A switched ramping rate to 1A/min to 120 A
Thursday, March 09, 2023, 09:53
ramping at 4A/min (2A/30s) to 400A
IGP1= 9.9e-07 Torr
Thursday, March 09, 2023, 11:26
1130 am reaching 425A on TGHT
1850 C OMEGA
Thursday, March 09, 2023, 15:37
TGHT 425 A, 7.1V
OMEGA = 1850 C
Starting rampdown @ -2A/min
endcaps and spring looked really good.
|
Monday, March 06, 2023, 21:34, Darwin Ortiz Rosales, SiC, 44692-3, HP-SIS, Done, 230306SiC conditioning
|
Monday, March 06, 2023, 21:29
Total number of foils:382 ( including 5 analysis discs on the right side of the container)
Total length packed 17 cm (excluding 5 analysis discs that will be removed)
container has 4 Ta heat shields (one inner only around fins)
No endcaps inserted to facilitate out-gassing
Ta coated spring at both ends
ramp to 500A @ 1A/min TGHT and to 230A on TBHT
max approx 700A on TGHT and 230A on TBHT (Omega slope set = 0.990)
Then temperature = 1800C
TBHT will be set fixed at 230 A (max). TBHT heated manually and automatically to max.
Good vac at 5.00 e -4 Torr
Bad vac at 5.00 e-2 Torr
IGP1= 3e-06 Torr at start of initial ramp.
Tuesday, March 07, 2023, 07:23
IGP1= 1.2e-05 Torr
OMEGA = 1288 C
Tuesday, March 07, 2023, 10:01
Will ramp to 715 A and keep there for 4 hours. OMEGA readings not reliable beyond this point due to coating on EVAP2 window.
Tuesday, March 07, 2023, 11:10
TGHT = 715A, 11.0V
TBHT = 230A, 3.2V
OMEGA = 1750 C (but not reliable)
Maintaining for 4 hours then will ramp down @ -2A/min TGHT and -1A/min TBHT
Wednesday, March 08, 2023, 07:27
Final IGP1= 1.3e-07 Torr (before shutting down pumps) |
Saturday, March 04, 2023, 08:34, Darwin Ortiz Rosales, TiC, 44692-7, LP-FEBIAD, Done, TiC230301 conditioning
|
Saturday, March 04, 2023, 08:29
Ta LP-FEBIAD with 369 discs plus 5 removable discs wrapped with 3 Ta heat-shields (in layers)
Evap 2 will be pumped down over previous night
Desired temperature = 1500 C as in Elog #52 , TGHT will be ramped up to 300 A and then adjusted manually to 1500C if temperature readings are ok
otherwise will use plot from coating sintering to approximate 1500C.
TBHT will be set fixed at 230A (max).
Good vacuum = 5.00 e-4 Torr
Bad vacuum = 5.00 e-2 Torr
IGP1= 3.4 e-07 Torr
Start autoramp @2A/min to 80 A then autoramp heat @1A/min to 230 A (both TGHT and TBHT)
Then autoramp TGHT to 300 A
-
Saturday, March 04, 2023, 22:27
At 332 A, 5.6V on TGHT, 230 A, 3.3 V TBHT
OMEGA = 1370 C
Will autoramp to 375A on TGHT @0.25A/min then leave for 4 hours at 1500C
Cooling should start at 6 am march 5th
OMEGA reading 1498 @ 2 am
Sunday, March 05, 2023, 06:03
OMEGA reading 1442 C @550am
ramped up to 394 A on TGHT and OMEGA reads 1500 C
will leave for 40 minutes than test ramp up to observe outgassing
d until 715 am then begin rampdown.
Sunday, March 05, 2023, 07:22
ramped to 425 to test further outgassing temperature increase observed but only while increasing current.
OMEGA = 1590 C
TGHT= 425A, 7.6V
TBHT= 230A, 3.3V
IGP1=2.0e-06 Torr
ramping down @-2A/min on TGHT and -1A/min TBHT
|
Wednesday, March 01, 2023, 21:49, Darwin Ortiz Rosales, Ta, 44692-3, HP-SIS, Done, TaC coating sintering
|
Wednesday, March 01, 2023, 21:46
Ta HP-SIS was coated with TaC and wrapped with Ta heat-shields (3 layers + 1 inner layer around fins)
Desired temperature = 1850 C , TBHT will be set fixed at 230A (max).
Evap 2 will be pumped down over previous night
OMEGA slope= 0.990
Good vacuum = 5.00 e-4 Torr
Bad vacuum = 5.00 e-2 Torr
IGP1= 5.7 e-07 Torr
Start autoramp @1A/min to 500 A on TGHT and 230A TBHT.
Thursday, March 02, 2023, 10:10
ramping to 600A on TGHT @ 2A/30s, TBHT at 230A, 3.2V
Thursday, March 02, 2023, 11:22
At 11 am reached 1800s C and 1851C @1120 am.
TGHT = 690 A, 10.5V
TBHT = 230 A, 3.3V
Cool down to start at 3 pm
|
Tuesday, February 28, 2023, 07:21, Darwin Ortiz Rosales, Ta, 44692-7, LP-FEBIAD, Done, TaC coating sintering
|
Tuesday, February 28, 2023, 07:19
Ta LP-FEBIAD was coated with TaC and wrapped with Ta heat-shields (4 layers)
Desired temperature = 1850 C , TBHT will be set fixed at 230A (max).
Evap 2 will be pumped down over previous night
OMEGA slope= 0.990
Good vacuum = 5.00 e-4 Torr
Bad vacuum = 5.00 e-2 Torr
IGP1= 1.2 e-06 Torr
Start autoramp @1A/min to 80 A then autoramp heat @1A/min to 150 A. Then autoramp TGHT to 400 A and TBHT to 230A.1
Tuesday, February 28, 2023, 15:39
Will ramp to 426A to 1850C as per regression line.
Tuesday, February 28, 2023, 15:57
Will start cooling at 8 pm
OMEGA= 1858 C
IGP1= 2.12e-06 Torr
TGHT =426 A, 7.5 V
TBHT = 230 A, 3.2 V
Tuesday, February 28, 2023, 19:58
OMEGA = 1858 C
IGP1 = 1.04e-06 Torr
TGHT =426 A, 7.6 V
TBHT = 230 A, 3.2 V
rampdown TGHT at -2A/min and TBHT @ -1A/min
|
Thursday, February 23, 2023, 18:24, Darwin Ortiz Rosales, TaC, 45441-2, HP-FEBIAD, Done, TaC coating sintering
|
Thursday, February 23, 2023, 18:20
Ta HP-FEBIAD was coated with TaC and wrapped with Ta heat-shields (3 layers) and 1 under layer that doesn't cover the middle section.
Desired temperature = 1800 C , TBHT will be set fixed at 230A (max).
Evap 2 will be pumped down to 5e-06 Torr range
OMEGA slope= 0.990
Good vacuum = 5.00 e-4 Torr
Bad vacuum = 5.00 e-2 Torr
IGP1=2.5 e-06 Torr
Start autoramp @1A/min to 80 A then autoramp heat @1A/min to 150 A. Then autoramp TGHT to approx 675A and TBHT to 230A.1
Friday, February 24, 2023, 09:10
heated overnight @0.5 A/min to 400 A. Then started heating at 1A/min to 600 A while taking readings for current/Temp regression.
regression so far points to 682A to get to 1800C. Will continue taking readings and possible heat to 1850 C.
Friday, February 24, 2023, 09:43
autoramping to 690A at 1A/min
Friday, February 24, 2023, 11:24
ramping manually to 690A from 650A
Friday, February 24, 2023, 11:32
4 hours at 330pm
TGHT 492A, 10.6V
TBHT = 230A, 3.2V
IGP1=5.11e-06 Torr
OMEGA =1840 C
Friday, February 24, 2023, 15:36
TGHT = 692A, 10.6V
TBHT = 230 A, 3.2V
OMEGA = 1835 C
IGP1= 2.4e-06 Torr
Starting rampdown at -2A/min TGHT and -1A/min TBHT |
Thursday, February 09, 2023, 09:49, Darwin Ortiz Rosales, Nb, , TARGET BOAT, Done, condition Nb samples (Phillip)
|
Thursday, February 09, 2023, 09:47
Target boat with a layer of niobium foil on the bottom is used to heat up Nb samples to 1400 C for 4 hrs.
The niobium samples are wrapped in a Nb foil.
Boat is wrapped with 2 layers of Ta foil, careful to avoid touching samples.
Samples left in Evap2 overnight (pumping down).
Good vacuum = 5.0e-04 Torr
Bad vacuum = 5.0e-02 Torr
Thursday, February 09, 2023, 09:48
IGP1= 6.19e-07 Torr
Autoramping to 100A @1A/min
Thursday, February 09, 2023, 09:57
Vacuum stable. ramp at 6A/min to 50 A instead
Thursday, February 09, 2023, 10:09
ramping at 2A/min to 100A
Thursday, February 09, 2023, 11:29
1400C on OMEGA reached @ 341A, 5.5V Will stop and watch until stable
Thursday, February 09, 2023, 15:29
OMEGA= 1408 C
IGP1= 7.97e-07 Torr
Start rampdown @ -1A/min |
Friday, December 16, 2022, 10:03, Darwin Ortiz Rosales, TaC, , TARGET BOAT, Done, TaC coated endcaps and spring sintering
|
4 TaC coated springs and 4 Tac coated caps loaded into a target boat.
Target boat wrapped in 4 Ta heatshields
Target boat type was with endcaps at both ends.
Left in Evap2 over previous night to depressurize.
Target temperature= 1850-1900C for 4 hours
Good vacuum = 5e-04 Torr
Bad vacuum = 5e-02 Torr
Friday, December 16, 2022, 10:01
Heated @1A/min to 100A on TGHT
Then heated 2A/min to 120A
Friday, December 16, 2022, 10:08
started autoramp @4A/min to 300A
Friday, December 16, 2022, 11:15
TGHT=450 A, 7.6 V
OMEGA= 1863 C
IGP1= 7.2e-06 Torr
Will keep for 4 hours
Monday, December 19, 2022, 10:30
Sintering was perfect. Repeat same configuration next time. |
Friday, December 02, 2022, 09:50, Darwin Ortiz Rosales, , 45220-12, TARGET BOAT, Done, Grahite disc conditioning 221130-Graphite
|
Friday, December 02, 2022, 09:46
297 graphite discs packed into a Ta tube wrapped in four heatshields.
Good vacuum 5.0e-04 Torr
Bad vacuum 5.0 e-02 Torr
Will be conditioned @ 2000 C for 5 hours and then for one hour at 10A greater than final current. Final current will be calculated from
regression.
IGP1= 5.7 e-07 Torr
ramping to 40A @ 2A/min TGHT
Friday, December 02, 2022, 20:59
Was ramped to 320A but the window must be coated because Temperature readings are drastically off. Will cool down and repeat on Monday after cleaning window. Will ramp down at -2A/min
OMEGA= 1360 C, expect much higher.
Tuesday, December 06, 2022, 10:58
ramp started at 4A/min . Initial pressure was 2.6 e-07 Torr
Tuesday, December 06, 2022, 12:45
OMEGA readings low (1290 @ 331A, 5.6V )
Will tap up until pressure bump observed.
Tuesday, December 06, 2022, 13:04
Pressure bump observed around 440 A, 7.9 V
IGP1= 8.4 e-06 Torr.
Current stopped and will keep at this current for 10 hours (11 pm rampdown)
Tuesday, December 06, 2022, 13:24
Ramped to 500A, Will leave at 500A for the rest of the conditioning.
Tuesday, December 06, 2022, 23:05
Starting rampdown at -2A/min
IGP1= 4.9e-07 Torr
TGHT= 500A, 9.3V
Wednesday, December 07, 2022, 09:43
Dismounting today.
IGP1 final = 9.6e-08 Torr
Wednesday, December 07, 2022, 13:29
Reinstalled in the evaporator. Window was not shaded. Will try heating to 500A once more.
ramp at 6A/min |
Thursday, November 24, 2022, 11:08, John Wong, TiC, , TARGET BOAT, Done, Synthesis of TiC fibrous disc (TiO2/PAN only)
|
Thursday, November 24, 2022, 11:01
Target container contains one disc of e-spun TiO2/PAN fibrous disc, (Ref sample P-134).
Sample will be heated to 1875C, similar to the previous process, see e-log ID#599.
TGHT will be autoramped to 350 A and monitor the conditions before ramping up further.
Good vacuum: 3e-5 Torr
Bad vacuum: 5e-5 Torr
Omega slope: 0.99
Initiate autoramp: 1 A/min
Chamber has been pumped down below 5.0e-6 Torr.
Friday, November 25, 2022, 08:38
TGHT reached to 348A/5.8V; temp is holding at 1600 C since 19:00 yesterday, see attachment#1.
Stepping up TGHT to 400A and continue to monitor.
Friday, November 25, 2022, 09:45
TGHT reached to 400A/6.8V; temp holding at 1758C. Pressure coming down from 6.6e-7 Torr.
Ramping up to 410A.
Friday, November 25, 2022, 12:28
TGHT reached 410A/7.08V. temp holding at 1790 C. Pressure coming down from 6.9e-7 Torr.
Ramping up to 430A.
Friday, November 25, 2022, 13:01
TGHT reached 430A/7.4V. Temp holding at 1837 C. Pressure coming down from 7.73e-7 Torr.
Ramping up to 440A.
Friday, November 25, 2022, 13:50
TGHT reached to 440A/7.6V. Temp holding at 1864C. Tapping TGHT to 444A (readback 443A - 449 A)/7.7V.
Desired Temp has reached, 1875 C. Will continue to hold on this temp over the weekend.
Sunday, November 27, 2022, 21:14
TGHT has been holding at 442A (lowered by 2 A on Fri to maintain 1875C). Temp increased to 1887C. Pressure at 2.5e-7 Torr.
See attachment#2 for plots/temp.
Initiated cooling at 1A/min.
|
Tuesday, November 22, 2022, 14:59, Darwin Ortiz Rosales, TaC, 45220-12, LP-SIS, Done, TaC coating sintering
|
Tuesday, November 22, 2022, 14:58
The coated container was wrapped in four Ta foil heatshields.
Target temperature on OMEGA= 1860-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230A
Final TGHT current= ~400A (adjustable)
Heating autoramp starged at 4A/min on both TGHT and TBHT to 40A
Then at 2A/min on both heaters to 120A.
Good vacuum = 5.0 e-02 Torr
Bad vacuum = 5.0E-04 Torr
leaving to pressure down.
Wednesday, November 22, 2022, 19:10
OMEGA = 1942 C @ 396A on TGHT
lowered to 386A to 1900 and left for 4 hours.
After four hours, started rampdown at-2A/min TGHT and -1A/min TBHT
|
Friday, November 18, 2022, 15:13, Darwin Ortiz Rosales, TaC, 45220-1, LP-SIS, Done, TaC coating sintering
|
Friday, November 18, 2022, 15:08
The coated container was wrapped in four Ta foil heatshields.
Target temperature on OMEGA= 1860-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230A
Final TGHT current= ~400A (adjustable)
Heating autoramp starged at 4A/min on both TGHT and TBHT to 40A
Then at 2A/min on both heaters to 120A.
Good vacuum = 5.0 e-02 Torr
Bad vacuum = 5.0E-04 Torr
leaving to pressure down over weekend
Sunday, November 20, 2022, 12:11
start heatup IGP1=1.63e-07 Torr
Sunday, November 20, 2022, 14:21
OMEGA= 1900 at 395A, 6.6V on TGHT
Will leave until 6;20 pm |
Thursday, November 17, 2022, 08:14, Darwin Ortiz Rosales, TaC, 44692-12, TARGET BOAT, Done, TaC coating sintering
|
Thursday, November 17, 2022, 08:11
The coated container was wrapped in four Ta foil heatshields.
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= N/A
Final TGHT current= ~400A (adjustable)
Heating autoramp starged at 4A/min on TGHT 40A
Then at 2A/min on both heaters to 120A.
Good vacuum = 5.0 e-02 Torr
Bad vacuum = 5.0E-04 Torr
IGP1 initial = 2.7e-07 Torr
Thursday, November 17, 2022, 10:41
OMEGA=1897C at 358A, 6.0V
Will ramp down at 230 pm
Thursday, November 17, 2022, 14:34
starting rampdown at -2A/min
OMEGA reads 1865C and IGP1=7.6e-07 Torr
|
Thursday, November 10, 2022, 07:40, Darwin Ortiz Rosales, TaC, 45220-13, LP-SIS, Done, TaC coating sintering
|
Thursday, November 10, 2022, 07:40
The coated container was wrapped in four Ta foil heatshields.
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230A
Final TGHT current= ~400A (adjustable)
Heating autoramp starged at 4A/min on both TGHT and TBHT to 40A
Then at 1A/min on both heaters to 120A.
Good vacuum = 5.0 e-02 Torr
Bad vacuum = 5.0E-04 Torr
IGP1 initial = 2.8e-07 Torr
Thursday, November 10, 2022, 10:31
TGHT 230A 3.4V and TBHT at 230A , 3.9V
Continue ramp up for TGHT at 4A/min (2A/30s) to 380A
Thursday, November 10, 2022, 11:30
OMEGA =1886 C @ 430A, 7.1V TGHT; will leave for 4 hours
Thursday, November 10, 2022, 15:43
rampdown at -2A/min TGHT and -1A/min TBHT |
Monday, November 07, 2022, 14:26, Darwin Ortiz Rosales, TaC, 44139-4, TARGET BOAT, Done, TaC coating sintering
|
Monday, November 07, 2022, 14:24
The coated container tube was wrapped in four Ta foil heatshields.
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final TGHT current= ~400A (adjustable)
Heating autoramp starged at 4A/min to 40A
Then at 1A/min on both heaters to 120A.
Good vacuum = 5.0 e-02 Torr
Bad vacuum = 5.0E-04 Torr
IGP1 initial = |
Tuesday, November 01, 2022, 17:35, John Wong, TiC, , TARGET BOAT, Done, Np-TiC fibres systhesis
|
Tuesday, November 01, 2022, 17:24
2 samples of np-TiO2/C fibres were produced using the e-spinner. Each sample was wrapped with a piece of graphite sheet, and then loaded into a target container.
Sample will be heated to 1700 C.
TGHT will be autoramped to 450 A; this should be close to 1600 C. (see elog#596)
Good vacuum: 3e-5 Torr
Bad vacuum: 5e-5 Torr
Omega slope: 0.99
Initiate autoramp: 1 A/min
Chamber has been pumped down below 4.2e-6 Torr.
Tuesday, November 01, 2022, 22:46
Pressure currently at 6.4e-7 Torr.
Initiated auto-ramping
Wednesday, November 02, 2022, 09:37
TGHT was ramped up to 448A (readback 445-452A / 8.05V - 8.11V). The voltage is much higher than the last process, see elog #596.
Temperature is much higher at this current, reading at 1870 - 1872 C.
Will keep at this setting for now and continue to monitor.
See attachment#1 for the TGHT-Pressure plot.
Wednesday, November 02, 2022, 21:35
Samples have been heated for over 16 hours; temp has been stabilized at 1875 C, vacuum at 7.3 e-7 Torr.
Initiated cooling at 1A/min.
Chamber will be vented tomorrow morning.
|
Friday, October 28, 2022, 07:59, Darwin Ortiz Rosales, TaC, 45220-6, LP-SIS, Done, TaC coating sintering
|
Friday, October 28, 2022, 07:58
The coated container was wrapped in four Ta foil heatshields.
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230A
Final TGHT current= ~420A (adjustable)
Heating autoramp starged at 4A/min on both TGHT and TBHT to 40A
Then at 1A/min on both heaters to 120A.
Good vacuum = 5.0 e-02 Torr
Bad vacuum = 5.0E-04 Torr
IGP1 initial = 4.5e-07 Torr
Friday, October 28, 2022, 10:50
after reaching 120A and leaving until pressure drop, autoramp at 2.5A/30s (5A/min) towards 400A TGHT and 230A TBHT.
Friday, October 28, 2022, 11:22
OMEGA= 1890 @ 412A, 7.1 V on TGHT
Leaving for 4 hours
|
Tuesday, October 25, 2022, 12:25, Darwin Ortiz Rosales, TaC, 44139-15-SK, LP-SIS, Done, TaC coating sintering
|
Tuesday, October 25, 2022, 12:18
Container wrapped in 4 Ta foil heatshields
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230A
Final TGHT current= ~420A (adjustable)
Heating autoramp started at 2A/min on both TGHT and TBHT to40A
Then at 1A/min on both heaters to 120A.
Good vacuum = 5.0 e-04 Torr
Bad vacuum = 5.0E-02 Torr
Wednesday, October 26, 2022, 07:07
IGP1= 7.5e-7 Torr
start ramp at 2A/min to 40A
Ramped at 1A/min to 120A then held until pressure drop. Then ramped @ 4A/min to 400A on TGHT.
Wednesday, October 26, 2022, 14:09
Manually rampted TGHT to 415A, 6.9V will hold for 4 hours
OMEGA reads 1870 C initially
Thursday, October 27, 2022, 09:44
was held for 5 hours due to technical issues but should be ok.
OMEGA @ time of rampdown = 1830C
Rampdown @-2A/min TGHT and -1A/min TBHT
IGP1= 3.5e-07 Torr
|
Tuesday, October 18, 2022, 13:59, Hannah Toy, TiC, Target boat (tube), TARGET BOAT, Done, Synthesis of TiC
|
Tuesday, October 18, 2022, 13:52
38 pieces of samples made of TiO2/C/PVP loaded into a target boat wrapped with 2 layers of Ta-heat shield.
Samples will be heated to 1700, 1800, 1900, and 2000 C
Some of the pieces will be removed after each target temperature
Target chamber has been pumping down and the current pressure reading is 6.62e-6 T
Tuesday, October 18, 2022, 14:12
TGHT will be autoramped to 250 A
Good vacuum: 3e-5 Torr
Bad vacuum: 5e-5 Torr
Omega slope: 0.99
Initiate autoramp: 1 A/min
|
Wednesday, October 19, 2022, 09:50, John Wong, TiC, Target boat (tube), TARGET BOAT, Done, Synthesis of TiC
|
Hannah Toy wrote: |
Tuesday, October 18, 2022, 13:52
38 pieces of samples made of TiO2/C/PVP loaded into a target boat wrapped with 2 layers of Ta-heat shield.
Samples will be heated to 1700, 1800, 1900, and 2000 C
Some of the pieces will be removed after each target temperature
Target chamber has been pumping down and the current pressure reading is 6.62e-6 T
Tuesday, October 18, 2022, 14:12
TGHT will be autoramped to 250 A
Good vacuum: 3e-5 Torr
Bad vacuum: 5e-5 Torr
Omega slope: 0.99
Initiate autoramp: 1 A/min
|
Wednesday, October 19, 2022, 09:42
TGHT has reached to 250A/3.95V, Temp at ~1100 C. (The archiver is currently not working; already contacted Control to look into it.)
Pressure reached below 4.9 e-7 Torr.
Auto-ramp to 300 A at 2A/min. Continue to monitor.
Wednesday, October 19, 2022, 10:24
TGHT reached to 300 A/4.89V. Temp at 1206 C.
Pressure went up slightly and came down after the TGHT setpoint was reached, see attachment#1.
Continue to auto-ramp to 350A at 2A/min.
Wednesday, October 19, 2022, 11:35
TGHT reached to 350A/5.8V. Temp at 1360C.
Pressure reached above 1e-6 Torr and came down after TGHT reached the setpoint.
Continue to auto-ramp to 400 A at 2A/min
Wednesday, October 19, 2022, 11:57
TGHT reached to 400 A/6.89V. Temp at 1485C.
Pressure went up to 3.3e-6 Torr and came down after TGHT reached the setpoint, see attachment#2.
A temp vs current plot has been generated (see shared folder \Hannah\) - est TGHT 480A to reach 1700 (T1).
Auto-ramp to 420 at 1A/min. Continue to monitor closely...
Wednesday, October 19, 2022, 13:01
TGHT reached 420A/7.23V, Temp at 1520 C.
Continue auto-ramping to 440A at 1A/min.
Wednesday, October 19, 2022, 13:42
TGHT reached 440A/7.65V. Temp at 1572 C
Continue auto-ramping to 460A at 1A/min.
Wednesday, October 19, 2022, 14:10
TGHT reached to 460A/8.10 V. Temp at 1628 C.
Tapping up TGHT to reach 1700 C
Wednesday, October 19, 2022, 15:33
TGHT was tapped up to 474A, Temp reached to 1700 C since 14:30.
Pressure is slowing coming down, currently at 1.4 e-6 Torr.
Will hold at this target current for a few hours.
Wednesday, October 19, 2022, 16:58
Temp went up slightly to 1713 C as the pressure is coming down.
Lower TGHT to 468A/8.45V to maintain the temp at 1700 C.
Wednesday, October 19, 2022, 19:55
Temp went up again to 1716 C, but this time the pressure also went up, see attachment#3. Not sure why the target got hotter... the voltage seems normal and consistent.
Lower TGHT to 462A/8.44V to maintain at 1700 C.
Continue monitoring...
Wednesday, October 19, 2022, 22:56
Temp went up another 10 C, to 1710 C, TGHT is holding at 462 A/8.48V. Notice the TGHT current readback is fluctuating between 458A - 463 A.
Initiated cooling.. 2A/min
Friday, October 21, 2022, 08:55
All the samples were taken out from the Evap on Thursday Oct 20. We decided to do so because there was not enough sample in each batch for XRD analysis. All the sample will be analyzed as treated at 1700 C.
See attachement #$ for the overall TGHT/Vac plot.
|
Monday, October 17, 2022, 11:32, Darwin Ortiz Rosales, TaC, 45220-2, LP-SIS, Done, TaC coating sintering
|
Monday, October 17, 2022, 10:03
The coated container was wrapped in 4 Ta foil heatshields. (The 4 shields appear to work well)
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230A
Final TGHT current= ~420A (adjustable)
Heating autoramp started at 2A/min on both TGHT and TBHT to40A
Then at 1A/min on both heaters to 120A.
Good vacuum = 5.0 e-04 Torr
Bad vacuum = 5.0E-02 Torr
Monday, October 17, 2022, 12:45
Autoramping @4A/min on both TGHT and TBHT to 400 and 30A respectively
Monday, October 17, 2022, 12:56
slowed ramp to 2A/min on both heaters as pressure was increasing too fast. (1A/30s).
Monday, October 17, 2022, 13:30
increased ramp rate to 4A/min on TGHT as TBHT is already at 230A
Monday, October 17, 2022, 14:16
leaving at TGHT : 393A, 6.5V ; TBHT 233A, 4.2V
OMEGA reads 1864C. Will start rampdown at 6:17 pm
Monday, October 17, 2022, 18:16
OMEGA read 1875C at max and now reads 1856C
starting ramp down at -2A/min TGHT and -1A/min TBHT
Final IGP1= 1.4e-06 Torr
Tuesday, October 18, 2022, 09:37
IGP1= 2.72e-7 Torr
Turning heaters off on epics and turning vacuums off. |
Thursday, September 29, 2022, 10:02, Darwin Ortiz Rosales, , 44139-3, TARGET BOAT, Done, 220926-Graphite conditioning in target tube
|
Thursday, September 29, 2022, 09:57
A Ta container tube was wrapped with 3 Ta heatshields.
338 graphite discs were loaded.
one Tantalum cup (modified to fit losely) was inserted on the front end along with a Ta spring.
on the backside there is no spring but four discs glued together with PVA
The system was left to establish vacuum over night.
Good vacuum set to5e-04Torr
Bad vacuum was set to 5e-2 Torr
Total weight of system including springs = 249.07 g
OMEGA slope = 0.99
The target will be heated to 2100 C, held there for 10 hours. The target Temperature vs Power will be tabulated and the current required to reach 2100 will be extrapolated to avoid using OMEGA at higher temperatures.
a) The target will be removed, weighed and inspected
b) If the target boat is still good, run again at 10A higher than previous for 2 hours.
c) The target will be removed, weighed and inspected
d) i) If the weight is the same or negligible, experiment ends
ii) if the weight has decreased and target still intact, repeat from step b and document all measurements and settings
Thursday, September 29, 2022, 10:04
IGP1= 1.4e-04 Torr
TGHT= 80.0 A, 1.0V
Will allow pressure to drop and then continue heating
Thursday, September 29, 2022, 10:20
IGP1= 7.9e-05 Torr pressure on downward trend
Start heating at 2A/min to 200A
The target started dropping in temperature as current increased. Suspected OMEGA issue.
Started cooling at -2A/min
Will continue next week.
Monday, October 03, 2022, 11:05
Upon inspection, the window though which the OMEGA laser travels was coated with dark precipitate (mostly a spot in the direct path of the laser).
Cleaned the window and started pumpdown.
Monday, October 03, 2022, 12:57
start heating @2A/20s = 6A/min because the target had previously been heated past additive evaporation point.
IGP1= 3.8e-06 Torr
Monday, October 03, 2022, 18:41
Will heat to 500A and leave for 10 hours. The regression shows too high current to reach 2100. Not reasonable. So will work with 500A as a baseline.
Tuesday, October 04, 2022, 06:52
Temperature @500 A read 1742C
maintained for 10 hours
start rampdown at -2A/min
OMEGA currently 1099C
Current = 500 A
Voltage =9.9 V
IGP1= 5.9e-7 Torr
Tuesday, October 04, 2022, 21:32
Quartz window was completely covered with graphite like dust. final weight after heating = 244.57 g (a couple of discs came loose and they were weighed separately and not included in the next heating).
weighted target and added one extra heatshield because it looked like a lot of heat was escaping. Will treat at 500A again for 2 hours. The extra heat-shield should provide hotter environment.
new initial weight = 254.24 g (don't have a balance with greater precision .
Wednesday, October 05, 2022, 07:42
IGP1= 3.8e-07 Torr
ramping to 280A @ 3A/min
Wednesday, October 05, 2022, 11:40
ramping to 350 @ 3A/min
Then ramp to 500A
500A at 12:50
Wednesday, October 05, 2022, 15:52
ramping down at -2A/min
Thursday, October 06, 2022, 09:27
IGP1= 1.8e-07 Torr
Will dismount and weigh, then decide how to proceed
according to second regression, second heating was ~2000 C. OMEGA not reliable after 1700 C in this case.
Thursday, October 06, 2022, 12:34
The final weight after the second heating was = 254.19 g
reinstalled target and cleaned quartz window.
will heat up to 510 A
Friday, October 07, 2022, 07:46
IGP1= 3.0 e-07 Torr
ramp at 2A/min to 500A. will pause to take data points for regression.
Friday, October 07, 2022, 13:05
Start rampdown after two hours at 500A, 10.3V
-2A/min
|
Thursday, September 22, 2022, 07:15, Darwin Ortiz Rosales, TaC, , TARGET BOAT, Done, TaC coated endcaps and spring sintering
|
Thursday, September 22, 2022, 07:13
Each endcap is separated with a disc of graphite foil and rolled into 3 packs of 4 within a foil envelope in a target boat.
There are also 2 coated springs
The boat is wrapped with 3-layers of Ta heatshields.
Chamber pumped down over previous night
Good vacuum = 5.0e-04 Torr
bad vacuum = 5.e-02 Torr
OMEGA slope = 0.99
Will ramp TGHT up to 40 A then autoramp to 400A at 1A/min.
Final desired temperature on OMEGA (tap)= 1800C
IGP1= 3.8e-7 Torr
Thursday, September 22, 2022, 10:08
TGHT= 168A,
IGP1= 4.7E-07=6Torr
Increased ramp to 2A/min
Thursday, September 22, 2022, 12:08
TGHT= 400A, 6.7V
OMEGA= 1604C
Continuing autoramp to 450A @2A/min
Thursday, September 22, 2022, 12:36
TGHT=450A, 7.7V
OMEGA=1700C
Tapping to 1800C manually
Thursday, September 22, 2022, 12:54
OMEGA = 1750C at 505A, 8.8 V
Tapped to 540A, 9.5V
Will leave there for two more hours
OMEGA= 1800+/- 10 C
Thursday, September 22, 2022, 15:00
TGHT = 540A, 9.3V
OMEGA= 1713
start rampdown at-2A/min
Friday, September 23, 2022, 09:49
IGP1= 4.0e-7 Torr
Will dismount container
Saturday, September 24, 2022, 09:10
Endcaps looked good. The front spring sintered onto container and not usable. signs of overheating.
|
Wednesday, September 14, 2022, 11:48, Darwin Ortiz Rosales, , , TARGET BOAT, Done, Grahite disc conditioning 220907G
|
Wednesday, September 14, 2022, 9:30
A Ta container tube was wrapped with 3 Ta heatshields.
322 graphite discs were loaded.
one Tantalum cup (modified to fit losely) was inserted on the front end along with a Ta spring.
A Ta spring was also installed on the back end to maintain the discs inside the tube.
The system was left to establish vacuum over night.
Good vacuum set to5e-03Torr
Bad vacuum was set to 5e-2 Torr
Total weight of system including springs = 249.63 g
Two Ta foils were installed on the copper heatshield facing the ends of the container.
The initial weight of the front Ta foil = 22.5 g
The initial weight of the back Ta foil will be determined by difference after cleaning =
OMEGA slope = 0.99
The target will be heated to 2100 C, held there for 10 hours. The target will be removed, the end Ta foils will be removed to analyses, new Ta end foils will be installed and the Target will be heated to 2100 plus 10 A higher than previous and left at that temperature for 2 hours.
Wednesday, September 14, 2022, 9:47
IGP1= 4.57e--7 Torr
initial Utoramp at 1A/10s to 80A and held at 80 amps until pressure good.
Wednesday, September 14, 2022, 11:54
Start autoramp at 1A/20s to 120A
Wednesday, September 14, 2022, 12:22
Autoramp at 1A/20s to 200A
Wednesday, September 14, 2022, 12:34
Autoramp increased to 2A/20s when TGHT = 154A
Wednesday, September 14, 2022, 13:46
Autoramping to 512A as projected current for 2100 C
Wednesday, September 14, 2022, 14:24
OMEGA = 1945 C @ 512A
Tapped to 540A, 10.5V and OMEGA = 2075. Will leave at this current and see Temperature behaeviour.
After 10 min OMEGA reads 2080C. Will start cooling at 12:20 am
Wednesday, September 14, 2022, 14:29
OMEGA = 2104C will ramp down slightly to keep 2100C
Wednesday, September 14, 2022, 14:31
OMEGA = 2098 @ 530A, 10.4V
Wednesday, September 14, 2022, 14:33
OMEGA = 2100 @ 410A,9.8V
Wednesday, September 14, 2022, 14:45
OMEGA = 2093 at 500A, 9.75V
Wednesday, September 14, 2022, 15:07
497A, 9.6V, OMEGA 2100
Wednesday, September 14, 2022, 22:09
@ approximately 515 pm noticed that OMEGA was reading 1600 C while TGHT was at 497A and 10.0V
Suspect damage to the container and possible damage
Left at the same current.
Just now the OMEGA is reading 2200C at 497A and 9.7V. Out of precaution, lowered the current to 475A and the volatage is 9.2V
OMEGA now reads 2152 C. Will leave at this current until 12:30 am when the 10 hour heating will end and will start rampdown at -2A/min
Thursday, September 15, 2022, 00:05
TGHT= 475A, 9.2V
OMEGA= 2126 C
IGP1= 1.33e-6 Torr
lowered current to 470A, 9.1 V, IGP1= 1.3e-6 Torr, OMEGA stabilized at 2120C
Thursday, September 15, 2022, 00:09
IGP1= 1.3e-6 Torr
will increase 10A to see pressure response. OMEGA= 2130C
Increase in IGP1 to 1.4e-6 Torr observed but immediately started to trend down
Thursday, September 15, 2022, 00:16
IGP1= 1.36e-6 Torr
OMEGA = 2131A
TGHT = 480 A
Thursday, September 15, 2022, 00:18
Start ramp down at -2A/min
Thursday, September 15, 2022, 09:45
IGP1=4.35e-07 Torr
TGHT turned off
Starting dismounting of target tube
Thursday, September 22, 2022, 07:04
Container tube was crystalized and was easily cut with a small pair of nail scissors. All but 18 discs were transferred to a new container. WO# 44691-3 |
Thursday, September 01, 2022, 12:32, Darwin Ortiz Rosales, TaC, 44691-13, LP-SIS, Done, TaC coating sintering
|
Thursday, September 01, 2022, 10:34
The coated container was wrapped in three Ta foil heatshields.
Target temperature on OMEGA= 1850-1900 C
OMEGA slope:= 0.990
Target time at max temperature = 4 hours
Final Current TBHT= 230A
Final TGHT current= ~420A (adjustable)
Heating autoramp starged at 2A/min on both TGHT and TBHT to 40A
Then at 1A/min on both heaters to 120A.
Good vacuum = 5.0 e-05 Torr
Bad vacuum = 5.0E-04 Torr
Thursday, September 01, 2022, 12:39
Has been stabilizing at 40A on both heaters.
Starting 1A/min autoramp to 80A
A discrepancy between setpoint and readback currents was observed for both TGHT and TBHT. The difference is substancial and warrants investigation. This process will be paused until further notice
Tuesday, September 06, 2022, 14:45
Controls has been troubleshooting EVAP2. In the process TBHT has been damaged. Arthur will take a look at it ASAP and his group will try and fix it tomorrow.
Regarding our initial problem, it appears that when an electrical safety box was installed, the copper water lines connected to output terminals of the power supply, were moved so that they were in contact with the evaporator cage. See the figure below.
Thursday, September 08, 2022, 12:47
Target has been removed and a new test target (HP-FEBIAD) has been placed inside. System left to generate enough vacuum and then testing will be performed.
Friday, September 09, 2022, 15:58
System was tested and all seems good. This coat/sintering will continue after conditioning of graphite material
Saturday, September 24, 2022, 09:13
Continuation of process.
IGP1= 4.3e-07 Torr
ramping @ 1A/min to 230 A on both TGHt and TBHT
Saturday, September 24, 2022, 16:28
ramped to 430A, 7.2V on TGHT and 233A, 4.2V on TBHT. Will leave until 7 pm.
Saturday, September 24, 2022, 19:44
Starting rampdown @-2A/min TGHT -1A/min TBHT
camera offline
IGP1= 1.2e-6 Torr
Monday, September 26, 2022, 09:41
IGP1=2.2e-07 Torr. Shutting off TBHT and TGHT.
Thursday, September 29, 2022, 09:53
Final notes: coating looks good . Probably 3 hours at final temperature is better to prevent material degradation. |
Thursday, August 25, 2022, 10:16, Darwin Ortiz Rosales, TiC, 44692-10, HP-FEBIAD, Done, TiC 220818 Sintering (TiC #6)
|
Thursday, August 25, 2022, 10:06
Target container is loaded with 379 Discs of TiC for Target and 5 extra discs for analysis on left end
Target length = 12.5
3 Ta foil heatshields and on TaC coated Ta spring on right side
Total weight including heatshields and spring = 1551.4 g Final total weight = 1545.5 g
Final power should be ~10988 Watt
TGHT ramp up to 820A, and TGHT to 300A at 0.1A/min.
IGP1= 7.7e-7 Torr
Good vacuum =3.0e-05 Torr
Bad vacuum = 5e-04 Torr
Initial TGHT and TBHT autoramped @1A/min to 50A
TBHT mas 230A
TGHT max depends on final power
Thursday, August 25, 2022, 11:17
Start autoramp at 1A/min to 80A on both TGHT and TBHT
Thursday, August 25, 2022, 11:54
leaving at 80A until pressure stops rising
Thursday, August 25, 2022, 22:29
left to autoramp to 230A TBHT and 750 A TGHT since approximately 2:00 pm
Will leave ramping @1A/min to 750 A on TGHT
TBHT currently at 230A
Friday, August 26, 2022, 07:27
TGHT = 850A, 9.3V
Started autoramp to 850A at 1A/min for TGHT
TBHT held at 230A
OMEGA = 1584C
Friday, August 26, 2022, 09:34
Target running at ~820A, 13.1 V since 9
Cooling to start between 1:15 to 1:30 pm
OMEGA reads 1668 C at top current
current reading oscillates between 812A and 828A and 13.1V to 13.2V.
Monday, August 29, 2022, 12:21
Cooling at -2A/min for TGHT and -1A/min TBHT started on time on Friday August 26th.
Target remained under vacuum after cooling, over the weekend.
Target removed this morning and looks good. 5 discs removed for analysis
|
Wednesday, August 10, 2022, 09:31, Ivan Bao, Empty, , TARGET BOAT, In progress, TC tests
|
1st test polarity 1
10:12 am Begin pumping down to rough vacuum
12:50 pm begin ramping up towards 2000C. Ta tube only, welded thermocouple mount
3:08 Ta tube reached 2000C, began ramping down. The ramping up process was smooth and no hiccups happened
4:57 ramp down complete, began shutting down the evap2, will let the turbopump to slow down spin overnight.
2nd test polarity 2(swapped)
Tuesday, Aug 09 2022, 4pm begin pumping to vacuum after switching the polarity of the power supply
Wednesday, August 10, 2022, 13:09 begin ramping up
3:18 ramped to 671A. 2000C, no hiccups, everything is nominal. The thermocouple reads higher than before, about 20-30 deg C colder than pyro at high temperatures (1400C and above)
No bad connections, short circuits or unexpected overheating.
begin ramping down
ramping down was smooth, with error being the TC about 40 deg C colder than pyro at temp above 1500C
ramping done completed at Wednesday, August 10, 2022, 16:46 , shutting down evap 2 roughing and turbopump |
Thursday, August 04, 2022, 09:31, Ferran Boix Pamies, Empty, , TARGET BOAT, In progress, TC on Ta boat test.
|
11am: Setting up new target tube thermocouple test
Thursday, August 04, 2022, 09:31 Test finished August 3rd afternoon. Venting now.
|
Wednesday, June 29, 2022, 10:12, Darwin Ortiz Rosales, TaC, 44692-10, HP-FEBIAD, Done, TaC coating sintering
|
Wednesday, June 29, 2022, 10:07
Ta HP-FEBIAD was coated with TaC and wrapped with Ta heat-shields (3 layers)
Desired temperature = 1800 C , TBHT will be set fixed at 230A (max).
Evap 2 will be pumped down over previous night
OMEGA slope= 0.990
Good vacuum = 3.00 e-4 Torr
Bad vacuum = 5.00 e-2 Torr
IGP1= 1.2 e-06 Torr
Start autoramp @2A/min to 80 A then autoramp heat @1A/min to 150 A. Then autoramp TGHT to 675A and TBHT to 230A.1
Wednesday, June 29, 2022, 10:13
Chamber isolation performed and no change of pressure observed.
Water leak test performed and no pressure change detected.
Starting ramp up
Wednesday, June 29, 2022, 13:23
Ramping to 675A on TGHT and 230A on TBHT @ 2A/min
Ramped TGHT to 680A, 10.6V and held for 4 hours
Wednesday, June 29, 2022, 21:52
Started rampdown @-2A/min TGHT and -1A/min TBHT |
Tuesday, June 28, 2022, 09:31, Ferran Boix Pamies, Empty, 41882-2, TARGET BOAT, In progress, TC test on Ta tube
|
Tuesday, June 27, 2022, early afternoon: We assembled the setup in evap2 and started the pumps leaving it running over night.
Tuesday, June 28, 2022, 09:31 Turbo pump stopped for unknown reasons a few hours after we left. Restarting the pump.
Tuesday, June 28, 2022, 10:23 Vacuum down to 1e-5T start to ramp up TGHT 1A/10s to 200A.
Tuesday, June 28, 2022, 1:20 pm, Ramped from 0-500A. thermocouple reading 900C while pyrometer reads 1600C. begin ramping down to 0A. |
Tuesday, June 21, 2022, 09:48, Darwin Ortiz Rosales, SiC, 37978-1, HP-FEBIAD, Done, T-220617 sintering
|
Tuesday, June 21, 2022, 09:43
Total number of foils: 377 ( including 6 analysis discs on the right side of the container)
Total weight = 1454 g (includes heatshields, spring and T bar)
Total length packed 15.5 cm (excluding 6 analysis discs that will be removed)
container has 3 Ta heat shields and is coated
No endcaps inserted to facilitate out-gassing
Ta coated spring at front (right) side
Initially to ramp TGHT and TBHT to 80A at 2 A/min
then to 120A and slow down ramp when pressure begins to increase
max approx 675A on TGHT and 230A on TBHT (Omega slope set = 0.990)
Then temperature = 1800C
TBHT will be set fixed at 230 A (max). TBHT heated manually and automatically to max.
Good vac at 3.00 e -4 Torr
Bad vac at 5.00 e-2 Torr
IGP1=3.6 e-07 Torr at start of initial ramp.
Tuesday, June 21, 2022, 13:54
IGP1= 7.1 e-05 and dropping. Start ramp to 150A for both TGHT and TBHT @1A/min
Tuesday, June 21, 2022, 21:27
Increased ramp rate to 3A/min for TGHT to 675A
Tuesday, June 21, 2022, 22:38
Ramp up to 685 A on TGHT and leave for 4 hours.
OMEGA = 1645 C but suspect reading not on Ta surface.
Wednesday, June 22, 2022, 02:28
IGP1=7.7e-6 Torr
OMEGA =1610C
TGHT = 685A, 10.5V
TBHT = 230A, 3V
initiate rampdown at -2A/min and -1Amin TGHT and TBHT |
Monday, June 20, 2022, 14:52, Darwin Ortiz Rosales, Empty, , , Done, softstart of new TP
|
Monday, June 20, 2022, 14:50
A new Turbo pump was installed this morning and it was soft started. It has operated correctly and it is ready for use. Derek O. installed it.
Previous pump had issues at start-up and was diagnosed as finished by Edi/
|
Tuesday, June 14, 2022, 09:04, Darwin Ortiz Rosales, Ta, 37978-1, HP-FEBIAD, Done, TaC coating sintering
|
Tuesday, June 14, 2022, 08:47
Ta HP-FEBIAD was coated with TaC and wrapped with Ta heat-shields (3 layers)
Desired temperature = 1800 C , TBHT will be set fixed at 230A (max).
Evap 2 will be pumped down over previous night
OMEGA slope= 0.990
Good vacuum = 3.00 e-4 Torr
Bad vacuum = 5.00 e-2 Torr
IGP1= 1.2 e-06 Torr
Start autoramp @2A/min to 80 A then autoramp heat @1A/min to 150 A. Then autoramp TGHT to 675A and TBHT to 230A.
Tuesday, June 14, 2022, 08:49
IGP1= 0.13 Torr
*had timed out and it was off. I RST and turned back on.*
Will wait for the pressure to drop to start heating
Tuesday, June 14, 2022, 09:36
IGP1= 9.4e-06 Torr
Start autoramp @2A/min to 80A
Tuesday, June 14, 2022, 11:27
IGP1= 8.7 e-06 Torr Trending down.
TGHT= 146A, 1.6V
TBHT= 146A, 1.7V
Has been ramping at 1A/min
Change ramp rate to 2A/min to 700A on TGHT and 230A on TBHT
Tuesday, June 14, 2022, 14:48
Change final current on TGHT to 675A, according to plot. May change again.
Currently TGHT= 537A, 7.7V
IGP1= 4.4e-06 Torr
Tuesday, June 14, 2022, 18:46
Top temperature was 1825 Celsius at TGHT = 675A
Will start rampdown at 8:00 pm
Tuesday, June 14, 2022, 20:01
TGHT= 675A, 10.3 V
TBHT= 230A, 3V
OMEGA= 1815C
IGP1= 3.9e-06 Torr
ramping down @-2A/min TGHT and -1A/min TBHT |
Wednesday, June 08, 2022, 10:00, Flora Wu, , boat, , Done, carbonize PAN 10% discs
|
Thursday, June 09, 2022, 11:25
Total number of foils: 14 electrospun fiber pellets
Total weight = 208.3 g
container has 3 Ta heat shields.
Desired temperature at 1800 C
Omega slope set at 0.990
Good vac = 3.0e-5 Torr,
Bad vac = 5.0e-5 Torr.
Pumping down in progress
Thursday, June 09, 2022, 11:25
chamber pumped down below 5e-5
initiate auto ramping, 1A/min ----> 100 A
(see eLog 581)
|
Thursday, June 09, 2022, 19:20, John Wong, , boat, , Done, carbonize PAN 10% discs
|
Flora Wu wrote: |
Thursday, June 09, 2022, 11:25
Total number of foils: 14 electrospun fiber pellets
Total weight = 208.3 g
container has 3 Ta heat shields.
Desired temperature at 1800 C
Omega slope set at 0.990
Good vac = 3.0e-5 Torr,
Bad vac = 5.0e-5 Torr.
Pumping down in progress
Thursday, June 09, 2022, 11:25
chamber pumped down below 5e-5
initiate auto ramping, 1A/min ----> 100 A
|
Thursday, June 09, 2022, 19:16
Pressure came down below 10e-5 Torr as TGHT ramped up to 100A.
Continue auto ramping to reach 250A at 1A/min.
Thursday, June 09, 2022, 22:52
TGHT is hovering around 127A/1.68 V due to erractic pressure, see attachment #1.. Notice the backing line is at atm pressure - I don't recall this happened in the past.
Temp is still low to be detected on Omega. Will leave this overnight.
Friday, June 10, 2022, 09:07
TGHT has been holding at 250A/3.76V since 2:45am. Pressure comes down as THGT above 200 A. Backing line is back down normal.
Temp reading at 1040 C.
see attachment #2.
Continue to ramp up to 300A, monitoring temp/pressure.
Friday, June 10, 2022, 10:31
TGHT reached to 300A/4.63V, temp at 1145C. Pressure at 1.8e-6 and coming down.
Continue to ramp up to 350A.
Friday, June 10, 2022, 11:59
TGHT at 350A/5.66V, temp at 1300 C, Pressure at 8.1e-7 Torr, and coming down.
Continue to ramp up to 400A.
Friday, June 10, 2022, 13:19
TGHT reached to 400A/6.73V. Pressure coming down from 1.04e-6 Torr.
Temp at 1690. Will set up manually to reach 1800 C.
Friday, June 10, 2022, 13:50
TGHT stepped up to 432A/7.42V. Pressure coming down from 1.3 e-6 Torr.
Temp at 1800 C. See attachment#3 and #4 for the screenshot and temp-current plot.
Dumped striptool data to /usr1/evpr/carbonize_pan10_elog581_a and b.
Will keep at this setting over the weekend, and cooling down will take place on Sunday evening.
Sunday, June 12, 2022, 22:30
TGHT has been holding at 432A/7.40V since Friday. Temperature has gone up slightly to 1825.
See attachment#5 for the overall process.
Initiated cooling down at -2A/min.
Chamber will be vented on Monday morning.
|
Thursday, June 09, 2022, 09:09, Darwin Ortiz Rosales, Ta, , HP-FEBIAD, Done, Troubleshooting
|
Thursday, June 09, 2022, 09:07
Yesterday, Wednesday June 08, 2022 @ ~3.00 pm a "dummy" target container was installed in EVAP 2 after the heatshield assembly had been swapped.
The purpose is to test correct functioning of the system. Melting and evaporation on one of the bolts of the previous target container (eLog578) prompted the change in heatshield assembly and current testing.
TGHT was ramped up to 740A @ 4A/min, left to run at the final current for ~4.5 hours and then ramped down @-2A/min to 0A.
Will dismount dummy container this morning.
IGP1=2.5e-07 Torr
Thursday, June 09, 2022, 11:16
The target appears in good shape. No abnormal behaviour.
Picture attached are of the previous failed target eLog 578
|
Tuesday, June 07, 2022, 07:31, Darwin Ortiz Rosales, SiC, 42464-2, HP-FEBIAD, Done, T-220524 Sintering SiC
|
Tuesday, June 07, 2022, 07:19
Total number of foils: 403 ( including 5 analysis discs on the right side of the container)
Total weight = 1535.3 g (includes heatshields, spring and T bar)
Total length packed 16.4 cm (excluding 5 analysis discs that will be removed)
container has 3 Ta heat shields.
No endcaps inserted to facilitate out-gassing
Ta coated spring at front (right) side
Initially to ramp TGHT and TBHT to 50A at 3 A/min
then continue to 80A and slow down ramp when pressure begins to increase
max approx 700A on TGHT and 230A on TBHT (Omega slope set = 0.990)
Then temperature = 1800C
TBHT will be set fixed at 230 A (max). TBHT heated manually and automatically to max.
Good vac at 3.00 e -4 Torr
Bad vac at 5.00 e-2 Torr
IGP1= 7.6 e-07 Torr at start of initial ramp.
Tuesday, June 07, 2022, 11:14
Ramping to 150A on TGHT and TBHT at 1A/min
Ramped TGHT and TBHT to 230A at 2A/min
Tuesday, June 07, 2022, 13:12
Ramping TGHT to 600A at 4A/min
TBHT at 230A, 3.0V
Tuesday, June 07, 2022, 16:41
TGHT= 740 A, 12.1V
TBHT= 232A, 3.0 V
OMEGA reading 1616C but questionable. Will leave for 4 hours at 740A top TGHT.
Wednesday, June 08, 2022, 22:15
Early Wednesday morning the left TGHT bolt was found damaged. The target leg was coated with bolt material rendering the Target inoperable.
The Heatshield assembly was swapped and surfaces cleaned. A "dummy" FEBIAD was installed to test if the system can withstand high current.
The system was pumped down and ramped to 740A on TGHT at 4A/min. It was then left at that current for 4 to 5 hours.
Currently starting rampdown at -2A/min to 0A.
Photos of the incident attached in *eLog 580*. IGP1= 5.7e-06 Torr
TGHT= 742A, 11.4V |
Thursday, June 02, 2022, 16:53, Aaron Schmidt, Ta, 44691-12, LP-SIS, In progress, Conditioning Ta#64
|
Ta#64 LP-SIS target description:
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.0254mm (0.0010") Measured.
Target density = 12.005 g/cm3
Target length = 3.35 cm
Total Mass = 40.2166 g [Incl foils + Ta wire on 6 packs]
Total mass w/ Target oven= 446 g (w/ end caps)
Discs in target are arranged as follows: 1pack / 75 singles / 1pack / 100 singles / 2packs / 100 singles / 1pack / 75 singles / 1pack
End caps installed (Not expanded). No Ta foil heat shield added
Final desired temperature = 1900C.
Thursday, June 02, 2022, 16:49: Roughing
Thursday, June 02, 2022, 17:02: OMEGA slope = 0.98.
Thursday, June 02, 2022, 17:10: TP1 on.
Thursday, June 02, 2022, 17:21: TP1 is up to speed. PS on.
Friday, June 03, 2022, 05:22: Auto-ramping TGHT / TBHT to 500 / 200 A @ 2 A per min. Vacuum @ 1.78e-06T.
Friday, June 03, 2022, 08:59: TGHT / TBHT @ 424 / 200 A. Vacuum @ 3.42e-06T. Temperature @ 1318 C. Auto ramp ongoing.
Friday, June 03, 2022, 09:40: TGHT / TBHT @ 500 / 200 A. Vacuum @ 4.47e-06T. Temperature @ 1469 C. Auto-ramping TGHT / TBHT to 580 / 230 A @ 2 A per min
Friday, June 03, 2022, 10:47: TGHT / TBHT @ 580 / 230 A. Vacuum @ 6.26e-06T. Temperature @ 1620 C. Auto-ramping TGHT to 600 @ 2 A per min
Friday, June 03, 2022, 11:08: TGHT / TBHT @ 600 / 230 A. Vacuum @ 6.54e-06T. Temperature @ 1655 C. Auto-ramping TGHT to 630 @ 2 A per min
Friday, June 03, 2022, 11:30: TGHT / TBHT @ 630 / 230 A. Vacuum @ 7.73e-06T. Temperature @ 1708 C. Auto-ramping TGHT to 650 @ 2 A per min
Friday, June 03, 2022, 11:45: TGHT / TBHT @ 650 / 230 A. Vacuum @ 8.32e-06T. Temperature @ 1748 C. Auto-ramping TGHT to 660 @ 2 A per min
Friday, June 03, 2022, 11:53: TGHT / TBHT @ 660 / 230 A. Vacuum @ 8.83e-06T. Temperature @ 1755 C. Auto-ramping TGHT to 670 @ 2 A per min
Friday, June 03, 2022, 12:05: TGHT / TBHT @ 670 / 230 A. Vacuum @ 9.03e-06T. Temperature @ 1780 C. Auto-ramping TGHT to 680 @ 2 A per min
Friday, June 03, 2022, 12:11: TGHT / TBHT @ 680 / 230 A. Vacuum @ 9.14e-06T. Temperature @ 1795 C. Auto-ramping TGHT to 700 @ 2 A per min
Friday, June 03, 2022, 12:23: TGHT / TBHT @ 700 / 230 A. Vacuum @ 9.50e-06T. Temperature @ 1822 C. Auto-ramping TGHT to 720 @ 2 A per min
Friday, June 03, 2022, 12:29: TGHT / TBHT @ 720 / 230 A. Vacuum @ 1.00e-05T. Temperature @ 1853 C. Auto-ramping TGHT to 730 @ 2 A per min
Friday, June 03, 2022, 12:36: TGHT / TBHT @ 725 / 230 A. Vacuum @ 1.04e-05T. Temperature @ 1860 C. Manually tap up TGHT to reach desired temperature
Friday, June 03, 2022, 13:04: TGHT / TBHT @ 760 / 230 A. Vacuum @ 1.07e-05T. Temperature @ 1901 C. Desired temperature reached
Friday, June 03, 2022, 13:13: Auto-cooling at 2 A per min.
Monday, June 06, 2022, 07:07: PS off. BV1 closed & TP1 off.
Monday, June 06, 2022, 08:47: Venting. |
Wednesday, May 18, 2022, 09:59, Darwin Ortiz Rosales, SiC, 44692-9, HP-FEBIAD, Done, T-220516 Sintering SiC
|
Wednesday, May 18, 2022, 09:46
Total number of foils: 415 ( including 10 analysis discs on the right side of the container)
Total weight = 1580 g (includes heatshields and T bar)
Total length packed 17 cm (including 10 analysis discs that will be removed)
container has 3 Ta heat shields.
No endcaps inserted to facilitate out-gassing
Ta coated spring at front (right) side
Initially to ramp TGHT and TBHT to 30A at 3 A/min
then continue to and slow down ramp when pressure begins to increase
max approx 700A on TGHT and 230A on TBHT (Omega slope set = 0.990)
Then temperature = 1800C
TBHT will be set fixed at 230 A (max). TBHT heated manually and automatically to max.
Good vac at 3.00 e -4 Torr
Bad vac at 5.00 e-2 Torr
IGP1= 7.1 e-07 Torr at start of initial ramp. Note, first real operation with new noisy Turbo Pump.
Wednesday, May 18, 2022, 10:18
Pressure increase observed starting around 60A. Ramped to 70 A and will leave until pressure stabilizes
After about 30 minutes pressure dropped so ramped up to 90 A @1A/min on both TGHT and TBHT
Wednesday, May 18, 2022, 11:37
pressure spike around 90A. will leave until pressure stabilizes
Wednesday, May 18, 2022, 12:54
start autoramp to 100A at 1A/min. IGP1= 1.4e-4 Torr
Wednesday, May 18, 2022, 13:15
autoramp to 150A @1A/min
Wednesday, May 18, 2022, 13:41
At 110A another spike in pressure. System waiting for good vacuum
Wednesday, May 18, 2022, 15:24
ramped to 150A on both TGHT and TBHT. Ramping to 200 A at @A/min for both TGHT and TBHT
currently IGP1= 2.0e-4 Torr
Wednesday, May 18, 2022, 15:33
Pressure still trending down; therefore will start ramp at 4A/min to 400 amp on TGHT and 230A to TBHT
Wednesday, May 18, 2022, 16:22
Increasing ramp to 4A/min on TGHT
Wednesday, May 18, 2022, 17:26
switched to 6A/min in 1A/10s increments on TGHT
Wednesday, May 18, 2022, 17:43
Set final current to 730 A as per regression attached.
Wednesday, May 18, 2022, 17:54
Final current on TGHT = 740A, 11.9 V
OMEGA = 1775 C
TBHT = 230A,
Will leave for 4 hours
Wednesday, May 18, 2022, 19:56
Temperature dropped so increased current to 755A for the remaining of the time.
Friday, May 20, 2022, 08:58
Final notes: The difference between initial and final mass was 6 g as expected. Slight coating on window of evaporator may explain apparent temperature drop. Next time will keep current at projected setting. The material looks good with slight overheating on the outer discs of left side.
|
Tuesday, May 10, 2022, 14:43, Aaron Schmidt, , , , Maintenance, Active TP removed / Swap / Slow start TP
|
Tuesday, May 10, 2022, 14:42: TV551 Varian. SN: 202311 (Slightly active from BL1A - will not cross contaminate. Field only - Tagged) was removed as it was meant to be a temporary fix. Replacement (Refurbished) pump is to be installed. (Tomorrow - Use slow start function as per vacuum group)
Thursday, May 12, 2022, 13:30: Agilent TP & hardware installed.
SN: IT21381010
Thursday, May 12, 2022, 13:41: Roughing.
Thursday, May 12, 2022, 13:46: Halt.
Friday, May 13, 2022, 07:05: Roughing.
Friday, May 13, 2022, 07:18: TP1 on.
Friday, May 13, 2022, 07:23: Up to 14 KRPM. Pause/Halted startup (Whining?). Slow start w/ vacuum group.
Process to perform a TP slow start:
- Hold both top buttons on the controller for about 3 seconds
- Right Yes/No left to continue.
- Advance to soft start - 20 min.
- Back to remote start & go.
Friday, May 13, 2022, 08:26: TP1 on w/ slow start.
Friday, May 13, 2022, 08:39: 13 KRPM & climbing.
Friday, May 13, 2022, 09:10: TP at full speed. 38 KRPM. 0.5A 9w. This pump whines, but is operating fine. Likely will switch again when another is available. (It appears to have been dropped, Noted by Edi. Likely when shipped)
Friday, May 13, 2022, 09:14: TP off. Slow start function off. Back to normal function. |
Monday, April 25, 2022, 08:31, Ferran Boix Pamies, Empty, Ta boat used for annealing, TARGET BOAT, Done, PEEK sample test 2
|
Setup in vacuum over the weekend.
Monday, April 25, 2022, 08:31 IGP1:6.7e-7T . Ramping up 1A/10s to 500A.
Monday, April 25, 2022, 10:05 500A reached, waiting 1h. TC at 50degC
Monday, April 25, 2022, 10:59 TC at 58degC. Ramping down 1A/10s to 0 A.
Monday, April 25, 2022, 13:37 TGHT at 0A , venting system. |
Thursday, April 21, 2022, 09:45, Darwin Ortiz Rosales, TaC, 42218-2, LP-IG-LIS, Done, TaC coating
|
Thursday, April 21, 2022, 09:43
TaC coated Target container was placed in Evaporator 2 yesterday and left pressuring down.
Ta Heatshields: 3
Target temperature on OMEGA = 1800-1850 C
OMEGA slope: 0.990
Target time at temperature = 4 hours
Target final TBHT current: 230A
Approximate final TGHT current: 420A (will adjust manually)
Heating autoramp started @ ~2A/min on both TGHT and TBHT
initial IGP1 = 9.3e-7 Torr
Thursday, April 21, 2022, 10:38
Pressure trending down after peak. Start autoramp at 1A/min to 50A on both TGHT and TBHT.
Thursday, April 21, 2022, 10:56
Pressure continues to decrease. Will ramp up faster @4A/min to 90A for both TGHT and TBHT.
Thursday, April 21, 2022, 11:07
Second peak has begun to form . Will keep at 90A awaiting stabilization
Thursday, April 21, 2022, 11:35
pressure stable. Continue to autoramp at 1A/min and if pressure stable increase ramp to 4A/min
Thursday, April 21, 2022, 11:49
small peak observed and stabilizing. Autoramp @ 6A/min to 400A on TGHT and to 230A on TBHT
Thursday, April 21, 2022, 12:35
Regression plot . 1800C should be reached ~1800C.
Thursday, April 21, 2022, 12:44
Target current reached.
OMEGA = 1762 C
Will manually bump current to 415 A
OMEGA = 1802 @ 415 A @ 12:51 pm
Thursday, April 21, 2022, 16:50
OMEGA=1823 C
IGP1= 2.9e-06 Torr
TGHT= 417 A, 7.2 V
TBHT= 232A, 3.0V
Rampdown will start at -2A/min for both TGHT and -1A/min TBHT
|
Sunday, April 17, 2022, 10:37, Ferran Boix Pamies, Empty, Ta boat used for annealing, TARGET BOAT, Done, PEEK samples heat test
|
Thursday, April 14, 2022, 10:36 Setup, PEEK samples installed on heatshield with TC. Pump down over the weekend.
Sunday, April 17, 2022, 10:37 Vacuum 3e-7T, ramp up TGHT 1A/10s to 500A
Sunday, April 17, 2022, 12:00 500A reached, waiting 1hour. TC at 42degC.
Sunday, April 17, 2022, 12:57 after 1h, TC at 45degC. Ramping down 1A/10s. Vacuum 2.7e-6Torr.
Sunday, April 17, 2022, 14:33 ramped down to 0A. Turning off turbo and venting. |
Tuesday, April 12, 2022, 13:41, Aaron Schmidt, , , , Maintenance, New Flex - line HS installed
|
Old HS sprang a leak in the copper tubing.
HS#44378-15
Tuesday, April 12, 2022, 13:35: Roughing.
Tuesday, April 12, 2022, 13:49: TP1 switched on.
Tuesday, April 12, 2022, 13:57: TP1 stable (green).
Tuesday, April 12, 2022, 14:10: Vacuum @ 3.71e-05T & dropping.
Tuesday, April 12, 2022, 14:11: HS waterline opened.
Tuesday, April 12, 2022, 14:12: Vacuum @ 3.32e-05T.
Tuesday, April 12, 2022, 14:22: Vacuum @ 2.19e-05T (Stable).
|
Wednesday, March 23, 2022, 10:52, Darwin Ortiz Rosales, TaC, 44692-9, HP-FEBIAD, Done, TaC coating
|
Wednesday, March 23, 2022, 10:49
Ta HP-FEBIAD was coated with TaC and wrapped with Ta heat-shields (3.5 layers) (two pieces around the fins only and 3 layers around the whole )
Desired temperature = 1800 C , TBHT will be set fixed at 230A (max). TGHT expected to reach desired Temperature @~700A
Evap 2 was pumped down over previous night
Good vacuum = 3.00 e-4 Torr
Bad vacuum = 5.00 e-2 Torr
IGP1= 1.2 e-06 Torr
Start autoramp @0.5 A/min to 60 A
Wednesday, March 23, 2022, 11:37
Increase autoramp to 1A/min to 60A for both TGHT and TBHT
Wednesday, March 23, 2022, 12:24
Pressure increasing at 60A so will leave at this current until pressure drops
Wednesday, March 23, 2022, 13:32
IGP1 = 2.9e-06 Torr
Will autoramp at 0.5A/min to 90A both TGHT and TBHT
Thursday, March 24, 2022, 16:35
1800C reached at 724A TGHT . TBHT @ 230A. Will keep at this temperature for 4 hours.
Thursday, March 24, 2022, 20:20
IGP1 = 6.9 e-06 Torr
OMEGA= 1828 C
TGHT = 724 A, 11.6 V
TBHT = 232.8 A, 3.1 V
Will start ramp-down at 2035 @ -2A/min TGHT and -1A/min TBHT
|
Wednesday, March 09, 2022, 06:27, Darwin Ortiz Rosales, TaC, 42464-2, HP-FEBIAD, Done, TaC coating/sintering
|
Wednesday, March 09, 2022, 06:25
Ta HP-FEBIAD was coated with TaC and wrapped with Ta heat-shields (3 layers)
Desired temperature = 1800 C , TBHT will be set fixed at 230A (max).
Evap 2 will be pumped down over previous night
Good vacuum = 3.00 e-4 Torr
Bad vacuum = 5.00 e-2 Torr
IGP1= 1.2 e-06 Torr
Start autoramp @1A/min to 60 A
Wednesday, March 09, 2022, 09:29
TGHT= 60 A 0.67 V
TBHT = 60A 0.59V
IGP1= 1.77e-6 Torr
autoramp @ 2A/min to 120 A and monitor (both TGHT and TBHT)
Wednesday, March 09, 2022, 10:19
IGP1 was increasing to fast. Manually lowered current to 105A on both TGHT and TBHT.
Will allow pressure to stabilize
Plant group requested maintenance work for EF12/13
Therefore, keeping system as is until further instructions from plant group.
Thursday, March 10, 2022, 15:18
Will resume ramp up to 120 A for both TGHT and TBHT @ 1A/min
IGP1= 6.4 e-07 Torr
Thursday, March 10, 2022, 15:30
Increase ramp rate to 2A/min
Thursday, March 10, 2022, 17:41
@ 245 A TGHT and 230A TBHT ramp back down to 100 A for both as OMEGA not displaying Temperature. Will need to go in tomorrow to fix OMEGA
Friday, March 11, 2022, 14:25
Ramping at 2A/min to 230A for both TGHT and TBHT
Friday, March 11, 2022, 15:17
IGP1= 1.23e-6 Torr
Continue Ramping TGHT @ 3A/min to 400 A keep TBHT at 230A
Friday, March 11, 2022, 22:22
@ TGHT 725 A 1800 C was reached on OMEGA
Kept there since 7:20 pm. Start rampdown at 11:20 pm.
Friday, March 11, 2022, 23:19
IGP1= 6.9e-6 Torr
OMEGA= 1805C
TGHT= 725 A, 10.9V
TBHT= 232A, 3.1V
Start rampdown at -2A/min on TGHT and -1A/min for TBHT
|
Tuesday, February 15, 2022, 12:37, Darwin Ortiz Rosales, Nb, , TARGET BOAT, Done, Nb annealing for Phillip
|
Wednesday, February 09, 2022, 06:55
Target boat with a layer of niobium foil on the bottom used to heat up Nb samples to 1400 C for 4 hrs.
OMEGA slope = 0.99
The niobium samples are wrapped in a layer of Nb foil.
Boat is wrapped with 2 layers of Nb foil.
Good vacuum 3.00e-02 Torr
Bad vacuum 5.00e-02 Torr
Autoramping TGHT at 2A/min to 200A, then monitor until desired temperature
Initial IGP1=6.0e-06 Torr
Tuesday, February 15, 2022, 12:44
Increasing ramp up to 3A/min to 220 A as pressure very stable
Tuesday, February 15, 2022, 14:04
ramped up manually to 1400C
IGP1 =3.9 e-06 Torr
TGHT = 340A, 5.5V
OMEGA = 1400 C
Tuesday, February 15, 2022, 14:21
Temperature on OMEGA up to 1413 C
Lowering current to 332A , OMEGA = 1400 +/- 5C
Wednesday, February 16, 2022, 11:43
On Tuesday February15, 2020 @18:04 started ramp down @-3A/min
|
Thursday, February 10, 2022, 08:58, Darwin Ortiz Rosales, SiC, , HP-FEBIAD, Done,
|
Thursday, February 10, 2022, 08:52
Total number of foils: 528 ( including 10 analysis discs)
Weight without springs = 1521.9 g (includes heatshields and T bar)
Total length packed 18.1 cm (including 10 analysis discs that will be removed)
container has 3 Ta heat shields.
No endcaps inserted to facilitate out-gassing
Ta coated spring at ends
Initially to ramp TGHT and TBHT to 50A at0.5 A/min
Then heat automatically heat to OMEGA ~1400 C , then continue to max 530A on TGHT and 230A on TBHT (Omega slope set = 0.990)
Then temperature = 1800C
TBHT will be set fixed at 230 A (max). TBHT heated manually and automatically to max.
Good vac at 3.00 e -4 Torr
Bad vac at 5.00 e-2 Torr
IGP1= 1.0 e-06 Torr at start of initial ramp
IGP1 = 5.7 e-06 Torr
TGHT = 50.0 A, 0.6 V
TBHT = 50.0A, 0.5 V
continue to ramp up at 0.5A/min to 200A
Friday, February 11, 2022, 07:59
IGP1=3.0e-07 Torr and stable
TGHT= 201A, 2.8V
TBHT = 201A, 2.6V
continue autoramp at 1A/min to 230A on TBHT and 450A on TGHT
Friday, February 11, 2022, 12:41
IGP1= 6.6e-05 Torr
TGHT= 450A, 6.5V
TBHT= 232A, 3.1V
OMEGA = 1258C
Allowing pressure to drop. Will continue ramp up when [pressure around 9-e-6 Torr
Friday, February 11, 2022, 13:59
IGP1= 2.4e-05 Torr
Will ramp up at 1A/min to 550A on TGHT
Friday, February 11, 2022, 15:54
IGP1= 2.4e-05 Torr
TGHT= 551.0A, 8.3V
TBHT=232A, 3.2V
OMEGA= 1426 C
ramp to 600 A @ 2A/min
Friday, February 11, 2022, 16:23
TGHT= 600.1A, 9.3V
TBHT= 232A, 3.2V
OMEGA = 1612C
ramp to 689 @2A/min to 1800 C as projected in regression plot attached
Friday, February 11, 2022, 21:20
Evap has been at 1800 +/- 20 C for 4 hours and 10 minutes
OMEGA 1802 C
TGHT = 689 A, 11.0V
TBHT=232.8 A, 3.26V
IGP1= 1.3e-05 Torr and stabilizing.
will start cool down at -2A/min TGHT and -1A/min TBHT
|
Wednesday, February 09, 2022, 08:08, Darwin Ortiz Rosales, Nb, , TARGET BOAT, Done, Nb annealing for Phillip
|
Wednesday, February 09, 2022, 06:55
Target boat with a layer of niobium foil on the bottom used to heat up Nb samples to 1100 C for 4 hrs.
OMEGA slope = 0.99
The niobium samples are wrapped in a layer of Nb foil.
Boat is wrapped with 2 layers of Nb foil.
Good vacuum 3.00e-02 Torr
Bad vacuum 5.00e-02 Torr
Autoramping TGHT at 3A/min to 180A, then monitor until desired temperature (based on eLog 550)
Initial IGP1=9.9e-07 Torr
Wednesday, February 09, 2022, 08:00
TGHT = 225 A, 3.2V
IGP1= 1.17e-06 Torr
OMEGA= 1100C +/- 12C fluctuations
Wednesday, February 09, 2022, 11:55
TGHT= 225 A, 3.3 V
IGP1= 9.7e-07 Torr
OMEGA=1100C +/- 10C fluctuations
Wednesday, February 09, 2022, 11:56
Start cooling @-2A/min |
Thursday, November 25, 2021, 14:00, Aaron Schmidt, , , , , Lower insulator replaced
|
The Helicoil had mostly pulled out of the old one.
Thursday, November 25, 2021, 13:58: Insulator replaced. EVAP 2 is ready for use with ISAC targets. |
Wednesday, November 10, 2021, 18:07, Aaron Schmidt, Ta, 44691-11, LP-SIS, In progress, Conditioning Ta#63
|
Ta#63 LP-SIS target description:
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.025mm
Target density = 15.38 g/cm3
Target length = 3.4 cm
Total Mass = 52.296 g [Incl foils + Ta wire on 6 packs]
Total mass w/ Target oven= 457 g (w/ end caps)
Discs in target are arranged as follows: 1pack / 75 singles / 1pack / 100 singles / 2packs / 100 singles / 1pack / 75 singles / 1pack
End caps installed (Not expanded). No Ta foil heat shield added
https://elog.triumf.ca/TIS/Target+Production/114
TBHT will be ramped up to 230A
TGHT will be ramped up to 600A +
Final desired temperature = 1900C.
OMEGA slope = 0.98.
Wednesday, November 10, 2021, 18:05: Roughing.
Wednesday, November 10, 2021, 18:14: Omega Laser set. On end cap / ok. Slope = 0.980
Wednesday, November 10, 2021, 18:24: Turbo pump on.
Wednesday, November 10, 2021, 18:25: RV1 valve hissing. Stop TP. Reset, open / close RV1 multiple times. Hissing stopped on its own. Won't affect the pump down, letting pressure out, not in. Will need to replace later.
Wednesday, November 10, 2021, 18:27: Turbo pump on.
Wednesday, November 10, 2021, 18:32: TP ok. PS on.
Thursday, November 11, 2021, 11:08: Vacuum @ 4.56e-07T. Auto ramping TGHT / TBHT to 580 / 230 A @ 2A per minute.
Thursday, November 11, 2021, 13:49: TGHT / TBHT @ 313 / 230 A. Vacuum @ 1.46e-06T. Temperature @ 1051 C. Auto ramp continues.
Thursday, November 11, 2021, 16:55: TGHT / TBHT @ 580 / 230 A. Vacuum @ 5.11e-06T. Temperature @ 1621 C. Auto ramp TGHT to 610 A @ 2 A per min.
Thursday, November 11, 2021, 17:13: TGHT / TBHT @ 610 / 230 A. Vacuum @ 6.54e-06T. Temperature @ 1670 C. Auto ramp TGHT to 630 A @ 2 A per min.
Thursday, November 11, 2021, 17:32: TGHT / TBHT @ 630 / 230 A. Vacuum @ 7.82e-06T. Temperature @ 1709 C. Auto ramp TGHT to 650 A @ 2 A per min.
Thursday, November 11, 2021, 18:49: TGHT / TBHT @ 650 / 230 A. Vacuum @ 7.40e-06T. Temperature @ 1758 C. Auto ramp TGHT to 665 A @ 2 A per min.
Thursday, November 11, 2021, 19:02: TGHT / TBHT @ 665 / 230 A. Vacuum @ 8.37e-06T. Temperature @ 1790 C. Auto ramp TGHT to 685 A @ 2 A per min.
Thursday, November 11, 2021, 19:22: TGHT / TBHT @ 685 / 230 A. Vacuum @ 9.56e-06T. Temperature @ 1830 C. Auto ramp TGHT to 700 A @ 2 A per min.
Thursday, November 11, 2021, 19:41: TGHT / TBHT @ 700 / 230 A. Vacuum @ 1.18e-05T. Temperature @ 1870 C. Manually tap up to 705 A
Thursday, November 11, 2021, 19:43: TGHT / TBHT @ 705 / 230 A. Vacuum @ 1.25e-05T. Temperature @ 1885 C. Manually tap up to 710 A
Thursday, November 11, 2021, 19:44: TGHT / TBHT @ 710 / 230 A. Vacuum @ 1.34e-05T. Temperature @ 1890 C. Manually tap up to 715 A
Thursday, November 11, 2021, 19:46: TGHT / TBHT @ 715 / 230 A. Vacuum @ 1.75e-05T. Temperature @ 1898 C. Manually tap up to 717 A
Thursday, November 11, 2021, 19:46: TGHT @ 717 A. Temperature @ 1901 C. Temperature reached.
Thursday, November 11, 2021, 19:48: Begin auto-cooling @ 2 A per min.
Friday, November 12, 2021, 06:13: PS off. TP1 off. |
Monday, November 08, 2021, 09:36, Darwin Ortiz Rosales, Endcaps, , TARGET BOAT, Done, Coating of Ta caps and Ta springs (8 caps and 2 springs)
|
Monday, November 08, 2021, 09:35
Two groups of 4 caps wrapped in graphite with graphite discs in between.
Two TaC coated springs at either end of the boat.
Target temperature = 1800 C
Expected around 430 TGHT
Good Vacuum 3e-03 Torr
Bad Vacuum 5e-02 Torr
Evap two was left pressuring down over weekend.
Monday, November 08, 2021, 09:35
Starting autoramp to 40 A at 1A/min
TGHT = 2.5e-07 Torr
Monday, November 08, 2021, 10:57
IGP1 = 8.5e -06 Torr and dropping
set autoramp to 50A at 1A/min
IGP1 1.0e-05 Torr and dropping
Set TGHT to autoramp to 90 A @ 1A/min and leave until pressure below 9e-06 Torr
Monday, November 08, 2021, 15:09
IGP1= 9.6e-06 Torr
Start autoramp to 400A at 2A/min
Monday, November 08, 2021, 17:37
TGHT = 377 A, 6.1V
OMEGA= 1234 C
Monday, November 08, 2021, 17:58
OMEGA = 1292 (cannot trust )
400A, 6.3 V
1.4 e-05 Torr
Autoramp @ 1A/min to 425A
Will heat to 425A and keep there for four hours
Monday, November 08, 2021, 22:02
TGHT=420A, 6.7V
IGP1= 7.0e-06 Torr
Start ramp down at -2A/min
|
Wednesday, November 03, 2021, 09:24, Darwin Ortiz Rosales, Empty, 44691-10, LP-SIS, Done, TaC coating/sintering
|
Ta tube was coated with TaC and wrapped with Ta heat-shields (3 layers)
Note: placed tantalum foil heatshield on both sides of the copper heatshield assembly.
Desired temperature = 1800 C (expected TGHT ~430 A), TBHT will be set fixed at 230A (max).
Evap 2 was pumped down yesterday
Good vacuum = 3.00 e-03Torr
Bad vacuum = 5.00 e-02 Torr
Wednesday, November 03, 2021, 09:27
Start autoramp at 1A/min to 40A on both TGHT and TBHT
IGP1 initial: 5.3 e-07 Torr
Wednesday, November 03, 2021, 10:22
IGP1= 1.1 e-05 Torr
TGHT = 40 A, 0.5 V
TBHT= 38.5 A, 0.41 V
Will keep while monitoring pressure at 0.5 A/min to 60A
Wednesday, November 03, 2021, 10:35
IGP1 pressure trending down
IGP1= 6.7 e-06 Torr
Start ramp up to 60A at 0.5A/min
Wednesday, November 03, 2021, 11:24
IGP1 2.6 e-06 Torr and trending down
Start ramp up to 400A on TGHT and 230A on TBHT at 1A/min
Wednesday, November 03, 2021, 13:28
IGP1= 1.4e-05 Torr and trending down slowly. Will increase ramp speed to 1.5A/min on both TGHT and TBHT to the same final current as before.
Wednesday, November 03, 2021, 15:56
IGP1= 2.1 e-05 Torr
TGHT = 400 A, 6.9 V
TBHT = 233 A, 4.1 V
OMEGA = 1645 C
Will manually ramp up to 1800 C
Wednesday, November 03, 2021, 16:43
TGHT = 450 A, 7.9 V
TBHT = 233 A, 4.1 V
OMEGA = 1770 C
IGP1 increasing in Pressure. Will leave for 4 hours at this current.
Wednesday, November 03, 2021, 20:48
IGP1= 1.0 e-05 Torr
TBHT= 233A, 4.1 V
TGHT = 450 A, 7.9 V
OMEGA = 1751 C
Starting ramp down at -2A/min on TGHT and -1A/min on TBHT
|
Monday, November 01, 2021, 07:39, Darwin Ortiz Rosales, Empty, 44508-3, LP-SIS, Done, TaC coating/sintering
|
Monday, November 01, 2021, 07:37
Ta tube was coated with TaC and wrapped with Ta heat-shields (3 layers)
Note* on the leading end of the assembly I placed tantalum foil heatshield similar to what I previously observed there. I believe it may impact temperature at the entrance of the container tube.
Desired temperature = 1800 C (expected TGHT ~430 A), TBHT will be set fixed at 230A (max).
Evap 2 was pumped down over the weekend
Good vacuum = 3.00 e-03Torr
Bad vacuum = 5.00 e-02 Torr
Monday, November 01, 2021, 07:39
Starting autoramp at 1 A/min to 40 A on both TGHT and TBHT
IGP1= 3.5 e-07 Torr
Monday, November 01, 2021, 09:08
IGP1= 1.6 e-06 Torr
TGHT = 40A, 0.99 V
TBHT = 39A, 1,2 V
Start autoramp @ 1A/min for both TGHT and TBHT to 400A and 230A respectively.
Monday, November 01, 2021, 14:33
OMEGA= 1545 C
TGHT = 354 A, 6.0 V
TBHT = 233 A, 4.8 V
IGP1= 1.7 e-05 Torr
increase ramp rate to 2A/min
Monday, November 01, 2021, 14:44
OMEGA= 1585C
TGHT = 367A, 6.3 V
TBHT = 233 A, 4.8 V
IGP1= 1.7 e-05 Torr
Monday, November 01, 2021, 14:49
OMEGA= 1604 C
TGHT = 377A, 6.5V
TBHT = 233 A, 4.8 V
IGP1= 2.1 e-05 Torr
Monday, November 01, 2021, 14:53
OMEGA= 1624C
TGHT = 384 A, 6.6V
TBHT = 233 A, 4.8 V
Monday, November 01, 2021, 15:00
OMEGA= 1660C
TGHT = 400 A, 6.8V
TBHT = 233 A, 4.8 V
IGP1= 2.4 e-05 Torr
Monday, November 01, 2021, 15:17
Initiate autoramp to 430A on TGHT @2A/min
Monday, November 01, 2021, 16:34
OMEGA = 1750 C
TGHT = 430 A, 7.3 V
Better heat insulation than before. Next time need to place a Ta heatshield at the other end on the copper assembly. Will raise T to 435 A and keep until 1930 hours.
Monday, November 01, 2021, 20:23
IGP1= 1.6 e-05 Torr
Omega = 1760 C
TGHT= 436 A, 7.4 V
TBHT = 232 A, 4.8 V
* Note: kept a approx 1 hour extra hoping that pressure would drop further
Started ramp down at -2A/min for TGHT and -1A/min for TBHT
Coating looks reasonably good.
|
Wednesday, October 27, 2021, 11:09, Darwin Ortiz Rosales, Ta, 44691-3, LP-SIS, Done, TaC coating/sintering
|
Wednesday, October 27, 2021, 11:07
Monday, October 25, 2021, 11:52
Ta LPSIS tube was coated with TaC and wrapped with Ta heat-shields (3 layers)
Desired temperature = 1900 C (expected TGHT ~430 A), TBHT will be set fixed at 230A (max).
Evap 2 will be pumped down over previous night
Good vacuum = 3.00 e-3 Torr
Bad vacuum = 5.00 e-2 Torr
Initial total weight = 464.8 g
Final weight after sintering =
Thursday, October 28, 2021, 07:46
IGP1= 7.4e-07 Torr
Initiating autoramp to 40 A on both TGHT and TBHT
ramp rate = 1 A/min
Will keep at 40A for approximately 1 hour or until pressure below 1e-05 Torr
Thursday, October 28, 2021, 09:41
IGP1= 1.9e-06 Torr TGHT = 40.3 A, 0.48 V TBHT = 39.0 A, 0.48V
Autoramp @ 1A/min to 100A on both TGHT and TBHT
Thursday, October 28, 2021, 12:57
IGP1= 1.1e-06 Torr
TGHT = 100 A, 1.3 V
TBHT = 100 A, 1.2 V
Start autoramp at 2A/min to 400 for TGHT and 230 for TBHT
The current from the plot (below) required to reach 1900 C seems too high.
Will take to 430 A as previous. The slope was chequed previously. Need to check OMEGA.
Thursday, October 28, 2021, 20:08
IGP1= 3.34 e-06 Torr
TGHT = 430A , 7.2 V
TBHT = 233A, 4.1V
OMEGA = 1628C
Start ramp down at -2A/min for TGHT and -1A/min for TBHT
|
44691-3 TaC coating |
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
TGHT |
|
TBHT |
|
|
Temperature (C) |
Current (A) |
|
|
|
|
|
|
|
|
|
|
|
|
Temperature ( C ) |
Voltage (V) |
Current (A) |
Voltage (V) |
Current (A) |
|
1900 |
512.88 |
|
|
|
|
|
|
|
|
|
|
|
|
1250 |
3.90 |
255.0 |
|
|
|
1700 |
434.06 |
|
|
|
|
|
|
|
|
|
|
|
|
1302 |
4.30 |
279.0 |
|
|
|
1800 |
473.47 |
|
|
|
|
|
|
|
|
|
|
|
|
1343 |
4.60 |
294.0 |
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
1423 |
5.10 |
325.0 |
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
1484 |
5.7 |
348.0 |
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
1555 |
6.2 |
377.0 |
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
Slope |
2.537 |
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
Y intercept |
598.66 |
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
R2 |
0.999 |
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
Monday, October 25, 2021, 11:53, Darwin Ortiz Rosales, TaC, 42218-4, HP-IG-LIS, Done, TaC coating/sintering
|
Monday, October 25, 2021, 11:52
Ta IGLIS tube was coated with TaC and wrapped with Ta heat-shields (3 layers)
Desired temperature = 1900 C (expected TGHT ~430 A), TBHT will be set fixed at 230A (max).
Evap 2 will be pumped down over previous night
Good vacuum = 3.00 e-3 Torr
Bad vacuum = 5.00 e-2 Torr
Initial total weight = 439.0 g
Final weight after sintering = 438.8 g
Tuesday, October 26, 2021, 07:18
IGP1= 9.2 e-07 Torr
Will ramp to 50A at 1A/min on both TGHT and TBHT.
Tuesday, October 26, 2021, 08:37
IGP1= 3.0 e-05 Torr
TGHT= 50.2 A, 0.6 V
TBHT = 49.4 A, 0.5 V
Will allow pressure to drop further then start further ramp up
Tuesday, October 26, 2021, 14:36
TGHT = 100 A, 1.3 V
TBHT = 99 A, 1.0 V
IGP1 = 3.e-5 Torr
ramp up TGHT to 400 A and TBHT to 230 A at 1.5 A/ min
Tuesday, October 26, 2021, 18:46
Will keep at 430A on TGHT and 230A on TBHT for 4 hours.
OMEGA reading = 1653 C is suspicious based on previous coating.
Tuesday, October 26, 2021, 23:05
TGHT = 430.5 A, 6.9 V
TBHT = 232.09A, 2.8 V
IGP1= 8.8e-06 Torr
Start cooling THGT at -2A/min and TBHT at -1A/min |
Thursday, October 21, 2021, 09:58, Darwin Ortiz Rosales, TaC, , TARGET BOAT, Done, Coating of Ta caps and Ta springs (10 caps and 2 springs)
|
Thursday, October 21, 2021, 10:02
10 TaC coated Ta caps, wrapped in graphite foil.
2 TaC coated Ta springs .
All mounted inside a target boat with enclosed ends.
Good vacuum = 3.0 e-3 Torr
Bad vacuum = 5.0 e-2 Torr
Will heat up to 1800-1900 C and keep at Temp for four hours
OMEGA slope = 0.990
*Note that the turbo pump has been replaced and this is the first EVAP2 operation after replacement*
Thursday, October 21, 2021, 10:03
IGP1= 1.6 e-06 Torr
starting ramp up at 2 amp/min to 30 A on TGHT
Thursday, October 21, 2021, 10:46
Ramping to 40 A at 2A/min and will keep there for 20 minutes.
Thursday, October 21, 2021, 11:19
IGP1= 1.2e-05 Torr and dropping
Start ramp up to 400 A at 0.5A/min
Thursday, October 21, 2021, 18:58
Started ramping at 3A/min to 468A on TGHT
Thursday, October 21, 2021, 20:15
Current at 468. Will keep there until pressure low enough.
Friday, October 22, 2021, 05:50
IGP1= 8.9 e-06 Torr
Start ramp down at -2A/min
Monday, October 25, 2021, 11:47
Upon examination the caps and springs did not appeared coated. The camera was not online so the current used was based on previous elogs. It may have evaporated TaC due to over temperature.
The materials will be cleaned, recoated and resintered. |
Wednesday, October 13, 2021, 08:35, Aaron Schmidt, , , , Problems, Troubleshoot - Pump down issues.
|
Swapped out the Cu gaskets for SS gaskets in the HS top lines. (x2)
Wednesday, October 13, 2021, 08:35: Roughing.
Wednesday, October 13, 2021, 08:50: Turbo pump on. TP Current 6.06-6.10A.
Wednesday, October 13, 2021, 08:59: TP maxed out at 3-4 KRPM, yet went "Green/On".
Wednesday, October 13, 2021, 09:00: Change FULL to Low setting. Restart. TP Current 6.15A.
Wednesday, October 13, 2021, 09:08: Timed out. Restarted from 5 KRPM.
Wednesday, October 13, 2021, 09:14: Stalling @ 5 KRPM. Stop TP. Contact vacuum group.
Monday, October 18, 2021, 09:03: Roughing. Reboot TP controller.
Monday, October 18, 2021, 09:25: Walkthrough soft start w/ vacuum group. TP timed out. Soft start failed.
Monday, October 18, 2021, 09:31: EVAP 2 vented. TP to be disconnected & removed.
Monday, October 18, 2021, 09:55: TP removed. Quick check, barely spins when spin by hand gently. Replacement or refurbishment needed.
500 lpm turbo pumps installed. TV551 Varian. SN: 202311 (Slightly active from BL1A - will not cross contaminate. Field only - Tagged)
Wednesday, October 20, 2021, 11:35: Roughing.
Wednesday, October 20, 2021, 11:52: TP on.
Wednesday, October 20, 2021, 11:59: TP at speed.
Wednesday, October 20, 2021, 12:02: Vacuum @ 6.13e-05T. Open HS waterline.
Wednesday, October 20, 2021, 12:03: Vacuum @ 5.63e-05T & dropping.
Wednesday, October 20, 2021, 12:04: Vacuum @ 5.32e-05T. TGHT PS on. |
Tuesday, September 14, 2021, 09:33, Darwin Ortiz Rosales, , 42218-5, LP-IG-LIS, Done, TaC coating/sintering
|
Tuesday, September 14, 2021, 09:32
Ta IGLIS tube was coated with TaC and wrapped with Ta heat-shields (3 layers)
Desired temperature = 1900 C (expected TGHT ~430 A), TBHT will be set fixed at 230A (max).
Evap 2 was pumped down over previous night
Good vacuum = 3.00 e-5 Torr
Bad vacuum = 5.00 e-4 Torr
IGP1= 1.12 e-06 Torr
Initiate manual ramp to 50 A @ 1A/min
Tuesday, September 14, 2021, 14:44
IGP1= 1.25e-06 Torr
TGHT = 50A, 0.58V TBHT = 49A, 0.56V
Start autoramp to 400 A TGHT and 230A TBHT @ 1A/min
Heated to 1880 C and held for 4 hours. Log info written down but could not be found in system later.
Coating proceeded without issues. |
Wednesday, September 08, 2021, 12:43, Darwin Ortiz Rosales, , 44139-8-SK, TARGET BOAT, Done, C Conditioning
|
Wednesday, September 08, 2021, 12:36
297 C discs were loaded onto a Ta tube wrapped in 3 Ta heatshields. (10 of which are analysis discs). They should be the first to be pushed out as they were loaded last.
The discs were loaded upside down to facilitate transfer to final container post conditioning.
a Ta foil disc was placed at the front end and a Ta spring at the back end of the tube.
The weight of the whole system is 254.4 g
Evap 2 was left to reduce pressure overnight.
Target temperature is 2000 C for five hours @ approx 450A
Good vacuum = 3e-2 Torr
Bad vacumm= 5e-2 Torr
Thursday, September 09, 2021, 08:46IGP1= 7.5 e-07 Torr
Will manually ramp up TGHT to 80 A
Thursday, September 09, 2021, 09:09
pressure began to rise at 50A so will leave at 50 A waiting for stabilization.
Current began to shoot up to rapidly, lowered current to 40A.
Thursday, September 09, 2021, 10:34
At IGP1= 1.3e-4 Torr manually increasing current again
Thursday, September 09, 2021, 12:52
IGP1= 8.6e-5 and dropping
TGHT = 60A, 0.87 V
Will begin autoramp to 120A at 1A/min
Thursday, September 09, 2021, 14:06
IGP1= 3.2e-05Torr
TGH T= 120A, 1.9V
Set autoramp to 1A/10s to 200A
Thursday, September 09, 2021, 14:57
IGP1= 1.5e-05 Torr
TGHT = 200A, 3.4V
Set Autoram to 2A/10s to 450A
OMEGA = 1249 C
At 258A OMEGA = 1420 C
continue ramp up at 2A/10s to 450
projected 2000 C is 454 A
Thursday, September 09, 2021, 16:10
Tapped up to 470 A and OMEGA 1993C. Will leave at this current because T may rise.
Thursday, September 09, 2021, 21:21
OMEGA 2011 C
IGP1 = 6.9e-06 Torr
Ramping down @ -1 A/min
Thursday, September 09, 2021, 17:27
Temperature kept around 2000 C by reducing current. It was reduced to 455A and Temperature stabilized . Time of ramp down will be 21:10 |
Thursday, September 02, 2021, 07:14, Darwin Ortiz Rosales, TaC, 44691-7, LP-SIS, Done, TaC coating/sintering
|
Thursday, September 02, 2021, 06:36
Ta tube was coated with TaC and wrapped with Ta heat-shields (3 layers)
Desired temperature = 1900 C (expected TGHT ~430 A), TBHT will be set fixed at 230A (max).
Evap 2 was pumped down over previous night
Good vacuum = 3.00 e-5 Torr
Bad vacuum = 5.00 e-4 Torr
IGP1=7.7e-07 Torr
Initiate autoramp to 50 A @ 1A/min
Thursday, September 02, 2021, 06:54
Stopped autoramp after reading email about EF-12 trip and compressed air issue. Reset to 0 A both TGHT and TBHT
Thursday, September 02, 2021, 12:01
Ispite of site compressed air issues, EVAP 2 has not tripped. Will manually increase current to40A for both TGHT and TBHT.
IGP1= 1.06 E-06 Torr.
Friday, September 03, 2021, 08:06
IGP1= 7.2e-07 Torr
TGHT= 43A, 0.5 V
TBHT= 41A, 0.48 V
Start autoramp at 1A/min to 90A on both TGHT and TBHT
Friday, September 03, 2021, 10:22
IGP1= 1.55 e-06 Torr
TGHT = 90.1 A, 1.1 V
TBHT= 90.0 A, 1.2 V
Continue ramp up at 1A/min to 400 A for TGHT and 230A for TBHT
Friday, September 03, 2021, 16:05
430A on TGHT will keep for four hours. OMEGA = 1856 C but according to regression should be 1900. will keep at this temp.
Friday, September 03, 2021, 21:11
OMEGA has been at 1875C for 4 hours. Will start ramp down @ -2A per minute for TGHT and -1A min for TBHT
TGHT = 430 A, 7.3 V (current actually fluctuates between 428 and 433 A since new power supply
TBHT = 233A, 4.0V (set to 230 but displays 233) |
Thursday, August 05, 2021, 11:18, Darwin Ortiz Rosales, SiC, 44691-2, LP-SIS, Done, Dr blade and non-Dr blade Material Experiment (sintering)
|
Thursday, August 05, 2021, 11:10
Total number of foils: 380
Total length packed 13.5 cm
container has 3 Ta heat shields.
No endcaps inserted to facilitate out-gassing
Two Ta discs at either end and three graphite discs as separators
[Left end [ blade--no blade--blade---no blade] Right end ]
Initially to ramp TGHT and TBHT to 50A at0.5 A/min
Then heat manually to OMEGA ~1400 C , ramping TGHT manually and automatically to reach 430A A (Omega slope set = 0.990)
Then temperature = 1800C
TBHT will be set fixed at 230 A (max). TBHT heated manually and automatically to max.
Good vac at 3.00 e -5 Torr
Bad vac at 5.00 e-5 Torr
Total weight into Evap2 =503.8 g
Friday, August 06, 2021, 11:33
IGP1= 8.3e-07 Torr
Start heating at 0.5 A/min on both TGHT and TBHT up to 50A
Friday, August 06, 2021, 22:34
IGP1= 7.0e-06 Torr
TGHT= 50.1 A, 0.6 V TBHT = 50.0A, 0.6V
Continue heating at 0.5A/min to 400A on TGHT and 230A on TBHT
Saturday, August 07, 2021, 10:11
Stopped autoramping. Will allow some time at 63 A on both TGHT and TBHT
Saturday, August 07, 2021, 12:19
IGP1= 1.9e-05 Torr
Manually increase TGHT and TBHT to 65 A
Saturday, August 07, 2021, 23:01
IGP1= 5.8e-06 Torr
TGHT= 64.5 A, 08V TBHT=64.6A, 0.8V
Ramp up manually while monitoring pressure
Sunday, August 08, 2021, 08:46
IGP1= 6.0e-06 Torr
TGHT = 69A, 0.85V TBHT = 69A, 0.90V
ramp up manually
Monday, August 09, 2021, 08:54
IGP1= 1.38e-05 Torr
TGHT= 90.0 A, 1.1V, TBHT= 90.0A 1.3V
Start autoramp at 0.5 A/min on both TGHT and TBHT to 400A and 230A respectively.
Changed bad vacuum to 5e-04 Torr
Monday, August 09, 2021, 21:37
IGP1= 6.6e-06 Torr
TGHT= 300.3 A, 5.0 V, TBHT = 233.0 A, 4.1V
Increase ramp rate to 2A/min for TGHT to 400 A,
OMEGA = 1430 C
Monday, August 09, 2021, 22:09
Will autoramp at 2A/min up to 424A as per regression line on attached file
Monday, August 09, 2021, 22:58
Temperature drop on OMEGA. Unexpected. Will lower current on TGHT to 418A and keep there for 4 hours. OMEGA may not be reliable
Tuesday, August 10, 2021, 3:16
IGP1=8.8e-07 Torr
TGHT = 414A, 7.5V TBHT = 233A, 4.1V
ramp down at -2A/min for TGHT and -1A/min for TBHT
Tuesday, August 10, 2021, 10:35
IGP1= 3.6e-07 Torr
Dismount
Some discs, especially end sections were coated with a golden layer. |
Wednesday, July 21, 2021, 16:45, Ferran Boix Pamies, Empty, , TARGET BOAT, Done, parasitic target thermal tests v2, foil measurement.
|
2021-07-21 4:44pm Vacumm at 1e-5Torr. Water cooling leak check ok.
2021-07-21 4:54pm ramping up TGHT to 200A 1A/10s.
2021-07-21 5:31pm 200A TGHT, TC 94degC pyro 1100degC. TC very low, ramping down and venting.
2021-07-22 5:00pm Parasitic prototype target installed, Vacuum 3e-5T, leak check ok. Power on HE of parasitic target.
2021-07-22 5:14pm vacuum 2e-5T. Ramping up container to 100A , 1A/10s.
2021-07-22 5:33pm vacuum 1e-5T. All good at 100A. Ramping up container to 200A , 1A/10s.
2021-07-22 5:54pm vacuum 8.2e-6T. All good at 200A pyro at 1100degC. Ramping up container to 300A , 1A/10s.
2021-07-22 6:15pm vacuum 7.6e-6T. All good at 300A pyro at 1420degC. Ramping up container to 400A , 1A/10s.
2021-07-22 6:36pm vacuum 8e-6T. All good at 400A pyro at 1700degC. Ramping up container to 500A , 1A/10s.
2021-07-22 6:57pm vacuum 1e-5T. All good at 500A pyro at 1960degC. Ramping up container to 553A , 1A/10s.
2021-07-22 7:13pm vacuum 1e-5T. All good at 553A pyro at 2100degC.
2021-07-22 7:36pm Ramping down 1A/10s.
2021-07-23 10:00am Venting. |
Wednesday, June 23, 2021, 17:48, Aaron Schmidt, Ta, 44691-4, LP-SIS, In progress, Conditioning Ta#62 (Replacement)
|
Ta#62 LP-SIS target description: (REPLACEMENT FOR 44139-10)
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.025mm
Target density = 14.29 g/cm3
Target length = 3.4 cm
Total Mass = 48.602 g [Incl foils + Ta wire on 6 packs]
Total mass w/ Target oven= 456 g (w/ end caps)
Discs in target are arranged as follows: 1pack / 75 singles / 1pack / 100 singles / 2packs / 100 singles / 1pack / 75 singles / 1pack
End caps installed (Not expanded). No Ta foil heat shield added
Wednesday, June 23, 2021, 17:46: Roughing.
Wednesday, June 23, 2021, 18:03: TP1 on.
Wednesday, June 23, 2021, 18:09: TP1 @ speed. Vacuum @ 1.53e-04T & dropping.
TBHT will be ramped up to 230A
TGHT will be ramped up to 600A +
Final desired temperature = 1900C.
OMEGA slope = 0.98.
Thursday, June 24, 2021, 07:38: PS on.
Thursday, June 24, 2021, 07:45: TGHT / TBHT tapped up to 10 A. Slope @ 0.98
Thursday, June 24, 2021, 07:46: Auto Ramping TGHT / TBHT to 350 / 150 A @ @ A per min.
Thursday, June 24, 2021, 10:47: TGHT / TBHT @ 350 / 150 A. Auto Ramping TGHT / TBHT to 580 / 230 A @ @ A per min. Temp @ 1120 C
Thursday, June 24, 2021, 12:59: TGHT / TBHT @ 580 / 230 A. Vacuum @ 8.24e-06T. Temp @ 1717 C. Auto-ramping TGHT to 600 A @ 2 A per min.
Thursday, June 24, 2021, 13:10: Vacuum @ 8.83e-06T. Temp @ 1758 C. Auto-ramping TGHT to 620 A @ 2 A per min.
Thursday, June 24, 2021, 13:21: Vacuum @ 1.0e-05T. Temp @ 1798 C. Auto-ramping TGHT to 645 A @ 2 A per min.
Thursday, June 24, 2021, 13:37: Vacuum @ 1.15e-05T. Temp @ 1845 C. Tap up TGHT to 650 manually.
Thursday, June 24, 2021, 13:45: Vacuum @ 1.21e-05T. Temp @ 1875 C. Tap up TGHT to 665+ manually.
Thursday, June 24, 2021, 13:47: Vacuum @ 1.34e-05T. Temp @ 1901 C. Tapped up TGHT to 677 manually. Desired temperature reached.
Thursday, June 24, 2021, 13:51: Auto-cooling @ 2A per min
Friday, June 25, 2021, 05:30: TP1 off. BP1 off.
Friday, June 25, 2021, 07:36: Venting. |
Friday, June 11, 2021, 08:41, Darwin Ortiz Rosales, Nb, , TARGET BOAT, Done, Nb treatment for Norman
|
Friday, June 11, 2021, 08:05
Target boat with a layer of niobium foil on the bottom is used to heat up Nb samples to 1100 C for 4 hrs.
OMEGA slope = 0.99
The niobium samples are wrapped in a layer of Nb foil.
Boat is wrapped with 2 layers of Nb foil.
Good vacuum 3.00e-02 Torr
Bad vacuum 5.00e-02 Torr
Autoramping TGHT at 2A/min to 50A then to 100A, then monitor until desired temperature
Initial IGP1= 9.4e-07 Torr
Friday, June 11, 2021, 09:59
TGHT = 200 A, 2.7V
IGP1= 9.8e-07 Torr
Tap to 1100C
Friday, June 11, 2021, 10:09
Temperature reached at 10:05 am.
TGHT = 224A, 3.1V
IGP1= 1.0e-06 Torr
OMEGA= 1100C +/- 10C fluctuations
Friday, June 11, 2021, 14:10
TGHT = 224A, 3.1V
IGP1= 9.2e-.07 Torr
OMEGA = 1100C +/- 10C fluctuations
Started rampdown at -3A/min
|
Wednesday, April 28, 2021, 11:57, Darwin Ortiz Rosales, SiC, 42218-7, HP-SIS, Done, sintering discs for SiC#41 (or back-up for #40)
|
Wednesday, April 28, 2021, 11:54
Total number of foils: 449 (not including analysis discs)
Total length packed 16.7 cm
5 extra analysis discs and 2 dr. Blade discs
container has 3 Ta heat shields.
No endcaps inserted to facilitate out-gassing
One Ta disc inserted at front end
Initially to ramp TGHT and TBHT to 50A at0.5 A/min
Then heat manually to OMEGA ~1400 C , ramping TGHT manually and automatically to reach 530A A (Omega slope set = 0.990)
Then temperature = 1800C
TBHT will be set fixed at 230 A (max). TBHT heated manually and automatically to max.
Good vac at 3.00 e -5 Torr
Bad vac at 5.00 e-5 Torr
Thursday, April 29, 2021, 10:09
IGP1 = 6.5 e-07 Torr
Start heating at 0.5 A/min to 50 A on both TGHT and TBHT
Thursday, April 29, 2021, 21:45
IGP1= 7.7 e-06
TGHT = 50.3A , 0.59 V
TBHT = 49.4 A, 0.56 V
Pressure is taking a while to equilibrate. Will wait a bit more to continue heating
Thursday, April 29, 2021, 23:49
IGP1 = 7.2 e-06 Torr
will start ramping at 0.5 A/min to 100 A
Saturday, May 01, 2021, 20:09
Friday, April 30, 2021, 08:19
IGP1 pressure higher than bad vacuum. Stopped autoramp. Will allow vacuum to come back down and restart ramp.
Saturday, May 01, 2021, 09:04
Yesterday the system had tripped. All pumps had turned off and the pressure was found at 0.005 torr
vacuum was restarted.
Current IGP1= 6.5e-07 Torr
Restarting heaters.
Autoramp at 0.5A/min to 20A on both TGHT and TBHT
Saturday, May 01, 2021, 10:48
IGP1=5.9e-7 Torr
TGHT = 20.0 A, 0.24V
TBHT = 20A, 0.20V
Autoramp at 0.5A/min to 40A both TGHT and TBHT
Saturday, May 01, 2021, 13:26
TGHT = 40.0 A, 0.47 V
TBHT= 39A, 0.44V
IGP1= 5.5 e-07 Torr
Autoramp at 0.5A/min to 60 A on both TGHT and TBHT
Saturday, May 01, 2021, 20:09
TGHT = 60.0 A, 0.72V
TBHT = 59.4 A, 0.69V
IGP1= 4.4e-07 Torr
Autoramp at 0.5A/min to 100 A on both TGHT and TBHT
Sunday, May 02, 2021, 18:30
IGP1= 1.7 e-06 Torr
TGHT =100A, 1.3V
TBHT = 99.9A, 1.3V
Autoramp both heaters at 0.25A/min to 120A and monitor
Sunday, May 02, 2021, 18:45
pressure increase to 4.1e-06 Torr. TBHT unexpectedly rose to 120A and was manually tapped back down to 104 A. Will keep both , TGHT and TBHT, at 104 A for a while.
Sunday, May 02, 2021, 19:50
Stepping at 0.5A/min to 105A then to 110 A on both TGHT and TBHT
Sunday, May 02, 2021, 22:10
Will leave both TGHT and TBHT at 110 A until pressure comes back down
currently IGP1= 1.3e-05 Torr
Monday, May 03, 2021, 09:35
IGP1= 2.2 e-06 Torr
Tapping TGHT and TBHT to 115A
Monday, May 03, 2021, 11:30
Tapping TGHT and TBHT to 120A @ 1A/min
Monday, May 03, 2021, 18:38
IGP1= 5.4e-06 Torr
TGHT = 130.3 A, 1.8 V
TBHT = 129.1 A, 1.8 V
Continue gradual ramping at 1A/min in increments of 5 A
Tuesday, May 04, 2021, 09:27
IGP1= 3.2e-5 Torr
TGHT = 400 A, 6.0V
TBHT = 232 A, 3.6V
OMEGA = 1104 C
waiting for pressure to drop then will continue heating
Tuesday, May 04, 2021, 17:27
TGHT = 420.1 A, 6.5V
TBHT= 232A, 3.6V
OMEGA = 1139 C
IGP1= 1.15e-5 Torr
will increase ramp up at 0.5A/min to 430A and hold (TGHT)
Tuesday, May 04, 2021, 22:43
TGHT= 430A, 6.6V
TBHT = 232.8A, 3.6V
OMEGA= 1157 C
IGP1=6.6e-6 Torr
Set Autoramp at 0.5A/min to 540 A (TGHT)
Wednesday, May 05, 2021, 08:09
IGP1= 7.5e-06 Torr
TGHT = 534 A, 8.5V
TBHT=232 A, 3.7 V
OMEGA = 1485
Continue ramp at 0.5A/min to to 600 A on TGHT
Wednesday, May 05, 2021, 15:07
IGP1=1.2e-5 Torr
TGHT=601A, 9.6V
TBHT= 232A, 3.7V
OMEGA =1600 C
ramp to 650A on TGHT at 0.5A/min
Wednesday, May 05, 2021, 20:05
Tapped TGHT to 694A, 11.4 V (manually)
TBHT= 232A, 3.7V
OMEGA = 1790 C
IGP1= 2.5e-05 Torr
Will monitor Pressure and temperature . Will start 4 hour count.
Wednesday, May 05, 2021, 22:03
OMEGA = 1765 C
TGHT = 694A, 11.5V
TBHT = 232A, 3.8 V
IPG1= 1.6e-05 Torr
Manually bumping TGHT to 700 A
|
Thursday, April 15, 2021, 18:33, Marla Cervantes, Ta, 44139-6-SK, TARGET BOAT, Done, Carbon penetration on Ta
|
Thursday, April 15, 2021, 18:24
Tantalum samples were loaded in a tantalum testing tube and installed in the EVAP2 to heat under vacuum for 3 days at 2000 degC (~500A, 4kW).
The temperature is measured with the Omega pyrometer (slope 0.98)
Some of the samples are in contact with graphite and enclosed with Ta caps, the other samples are not in contact with carbon.
The testing tube is wrapped with 3 Ta heat shields and is not TaC coated.
Thursday, April 15, 2021, 18:31
IGP1 = 4.5e-7 Torr
Good vacuum = 3e-2 Torr
Bad vacuum = 5e-2Torr
The TGHT will be ramped to 500A at 5A/min
Thursday, April 15, 2021, 20:00
Finished ramping
TGHT = 502 A, 8.22 V, Omega 2012 degC
Sunday, April 18, 2021, 20:38
After 3 days at ~2000 degC, TGHT was ramped at -2A/min to 0A |
Tuesday, April 13, 2021, 10:44, Marla Cervantes, Empty, NA (Ta- tube Eagle Alloys), , Done, Re-coat 4
|
Tuesday, April 13, 2021, 09:51
IGP1 = 2.5e-7 Torr
Tuesday, April 13, 2021, 10:17
The wire was heated in the same manner as the last three runs
From 0A to 7A the autoramp was set to 0.5A/min
At 8A the wire started the glow dimmly
Above 8A, the wire was heated manually at 0.5A until 15A where the step was changed to 1A,
the temperature was measured with the filament pyrometer every 2 A starting at 10A
At 42 A the step was changed to 0.5A until 44.5A, 4.61V (2120 °C), the wire was kept at that temperature for 6 hours.
After that time, the current was ramped to 0A at 0.5A/min. |
Thursday, April 08, 2021, 08:25, Aaron Schmidt, Ta, 44139-10, LP-SIS, In progress, Conditioning Ta#62 & Flex - line HS installed
|
Ta#62 LP-SIS target description:
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.025mm
Target density = 13.96 g/cm3
Target length = 3.4 cm
Total Mass = 47.461 g [Incl foils + Ta wire on 6 packs]
Total mass w/ Target oven= 445 g (w/ end caps)
Discs in target are arranged as follows: 1pack / 75 singles / 1pack / 100 singles / 2packs / 100 singles / 1pack / 75 singles / 1pack
End caps installed (expanded). No Ta foil heat shield added
TBHT will be ramped up to 230A
TGHT will be ramped up to 600A +
Final desired temperature = 1900C.
OMEGA slope = 0.98.
Thursday, April 08, 2021, 08:24: Roughing.
Thursday, April 08, 2021, 09:06: Vent & check. Roughed to only 20 T.
Thursday, April 08, 2021, 09:18: Roughing. Loose flange found. Left side wall / upper right.
Thursday, April 08, 2021, 09:34: TP1 on.
Thursday, April 08, 2021, 14:41: Vacuum @ 1.65e-06T. Waterline opened.
Thursday, April 08, 2021, 14:46: Vacuum ok. Power on. TGHT / TBHT to 20 / 15 A. Ok.
Thursday, April 08, 2021, 14:50: Auto-ramping TGHT / TBHT to 300 / 100 A @ 2 A per min.
Friday, April 09, 2021, 05:08: Vacuum @ 6.23e-07T. Temp @ 1195 C. Auto-ramping TGHT / TBHT to 400 / 150 A @ 2 A per min.
Friday, April 09, 2021, 06:01: Vacuum @ 9.64e-07T. Temp @ 1447 C. Auto-ramping TGHT / TBHT to 500 / 200 A @ 2 A per min.
Friday, April 09, 2021, 07:23: Vacuum @ 1.92e-06T. Temp @ 1671 C. Auto-ramping TGHT / TBHT to 600 / 230 A @ 2 / 1 A per min.
Friday, April 09, 2021, 08:40: Vacuum @ 3.96e-06T. Temp @ 1877 C. Auto-ramping TGHT / TBHT to 620 A @ 1 A per min.
Friday, April 09, 2021, 09:10: Vacuum @ 3.60e-06T. Temp @ 1915 C. Drop TGHT from 620 A to 610 A manually.
TGHT to 613 A manually.
Friday, April 09, 2021, 09:15: Vacuum @ 3.60e-06T. Temp @ 1902 C. TGHT / TBHT @ 613 A / 230 A. Desired temperature reached.
Friday, April 09, 2021, 12:08: Auto-cooling @ 1 A per min initiated.
Monday, April 12, 2021, 07:23: PS / Turbo pump / roughing pump off.
Monday, April 12, 2021, 08:03: Vented. |
Sunday, April 04, 2021, 16:09, Ferran Boix Pamies, Empty, 41882-2, TARGET BOAT, Done, parasitic target commissioning
|
2021-04-04 16:07 New container is in with heatshields, vacuum 8.6E-6 torr. leak check done. ramping up current, checking both pyrometer and TC, 1A/10s.
2021-04-04 16:49 200A TGHT 250degC on TC 1130degC on pyrometer. Too low on TC, ramping down and venting to reposition TC in the foil.
2021-04-04 18:00 TC was slightly broken, repaired now. Pumping chamber.
2021-04-04 18:41 ramping up to 200A 1A/10s.
2021-04-04 18:41 200A TGHT, TC 389degC pyro 1130degC. ramping to 400A 1A/10s.
2021-04-04 18:41 300A TGHT, TC 554degC pyro 1440degC.
2021-04-04 18:41 400A TGHT, TC 735degC pyro 1720degC. ramping to 600A 1A/10s.
2021-04-04 20:15 500A TGHT, TC 891degC pyro 1990degC
2021-04-04 20:15 553A TGHT, TC 975degC pyro 2129degC, ramping down.
2021-04-06 13:44 Parasitic target plus thermocouples were introduced in evap2 the day before and put under vacuum. IG1 3E-7 torr, leak check done. Putting some power into HE while ramping up container to 100A 1a/10s.
2021-04-06 14:06 20W on HE 100A on target container. Everything stable. Ramping up to 200A 1A/10s
2021-04-06 14:06 20W on HE 200A on target container. Everything stable. Ramping up to 300A 1A/10s
2021-04-06 14:06 20W on HE 300A on target container. Everything stable 4.6E-7 torr. Ramping up HE to 40W.
2021-04-06 14:06 40W on HE 300A on target container. Everything stable 4.6E-7 torr. Ramping up container to 400A 1A/10s.
2021-04-06 14:06 40W on HE 400A on target container. Everything stable 1E-6 torr. Ramping up container to 500A 1A/10s.
2021-04-06 15:52 35W on HE 500A on target container. Everything stable 1.6E-6 torr. Ramping up He to 65W.
2021-04-06 18:40 at 50W on HE one of them broke, system ramped down, vented, HE replaced, pumping down system again.
2021-04-07 10:38 HE at 70W, ramping up container to 200A 1A/10s. Vacuum 3.3E-7 torr.
2021-04-07 10:59 HE at 70W, 200A on container, ramping up container to 300A 1A/10s. Vacuum 3.9E-7 torr.
2021-04-07 10:59 HE at 65W, 300A on container, ramping up container to 400A 1A/10s. Vacuum 4.5E-7 torr.
2021-04-07 11:50 HE at 70W, 400A on container, ramping up container to 500A 1A/10s. Vacuum 7.8E-7 torr.
2021-04-07 11:50 HE at 65W, 500A on container, ramping up container to 553A 1A/10s. Vacuum 1.4E-6 torr.
2021-04-07 11:50 HE at 65W, 553A on container. All good, ramping down. 1A,10s. |
Tuesday, March 30, 2021, 19:49, Ferran Boix Pamies, Empty, 44139-7-SK , , Done, Parasitic target thermal tests
|
2021-03-30 7:48 Target loaded with parasitic target only. No container. Leaving under vacuum over night.
2021-03-31 13:43 Leak check performed. Water on. Need to vent system, electric connection disconnected.
2021-03-31 15:02 First test successfully finished. Venting to introduce container with radiating heating gun.
2021-04-01 14:58 Vacuum 3.5E-7 torr. Leak check done. Ramping up target heater to 100A at 1A/10s
2021-04-01 14:58 Vacuum 5E-7, 100A all ok. Temp foil 24.3DegC. ramping to 500A at 1A/10s.
2021-04-01 14:58 Temp of foil not increasing much. Probably issue with TC. ramping down at 1A/10s to vent and inspect.
2021-04-02 11:03 Target reinstalled, foil TC reinstalled. Vacuum 3E-7 torr. Leak check done. Ramping up container to 500A 1A/10s.
2021-04-02 13:07 Still isues with TC. Container ramped down at 1A/10s. Venting, brought heat gun to check TC.
2021-04-02 15:10 TC connection fixed, origin of issues. Vacuum down to 3E-5 torr. Ramping up container to 200A 1A/10s.
2021-04-02 18:32 TGTH 200A Tc temp 327.5degC. ramping up to 300A. 1A/10s.
2021-04-02 18:32 TGTH 300A Tc temp 500degC. ramping up to 400A. 1A/10s.
2021-04-02 19:17 TGTH 400A Tc temp 618degC. ramping down.
2021-04-03 13:37 Foil was changed, ramped up to 200A at 1A/10s, Temp TC 360degC. Ramping to 300A. Vac 8.6E-6 torr.
2021-04-03 13:59 300A Temp TC 580degC. Ramping to 500A, 1A/10s. Vac 7.6E-6 torr.
2021-04-03 14:36 500A Temp TC 836degC. Ramping to 600A, 1A/10s. Vac 9E-6 torr.
2021-04-03 14:36 600A Temp TC 960degC. Vac 1.1E-5 torr. Ramping down.
2021-04-03 19:00 After venting an opening the evap2, it was found that remaining from a past heat treatment where on the Tantalum container. The sublimation of the material coated the inner walls of the evap.2. Now cleaned.
|
Sunday, March 28, 2021, 11:24, Marla Cervantes, , NA (Ta-tube), , Done, Re-coat 3
|
Objective: Coating the inner surface of a tantalum tube to make a destructive test and use a reference for the tantalum boats coatings
Results: The tube was coated
Sunday, March 28, 2021, 11:23
No water leak
IGP1 = 2.3e-7 torr
Sunday, March 28, 2021, 16:10
The wire was heated in the same manner as the last three runs
From 0A to 7A the autoramp was set to 0.5A/min
At 8A the wire started the glow dimmly
Above 8A, the wire was heated manually at 0.5A until 16A where the step was changed to 1A,
the temperature was measured with the filament pyrometer every 2 A starting at 10A
At 42 A the step was changed to 0.6A until 42.6A, 4.38V (2020 °C), the wire was kept at that temperature for 90 min
After that time, the current was ramped down at 0.5A/min until ~20A when the current rampping was changed too 1A/min
|
Friday, March 26, 2021, 16:23, Marla Cervantes, Empty, 44489-7, , Done, Re-coat 2
|
Objective: Coating the inner surface of a tantalum tube to make a destructive test and use a reference for the tantalum boats coatings
Results:
Sunday, March 27, 2021, 11:23
No water leak
IGP1 = 3.7e-7 torr
Sunday, March 27, 2021, 16:10
The wire was heated in the same manner as the last three runs
From 0A to 7A the autoramp was set to 0.5A/min
At 8A the wire started the glow dimmly
Above 8A, the wire was heated manually at 0.5A until 16A where the step was changed to 1A,
the temperature was measured with the filament pyrometer every 2 A starting at 10A
At 42 A the step was changed to 0.6A until 42.6A, 4.38V (2020 °C), the wire was kept at that temperature for 90 min
After that time, the current was ramped down at 0.5A/min until ~20A when the current rampping was changed too 1A/min
|
Friday, March 26, 2021, 13:58, Marla Cervantes, Empty, 44489-6, , Done, Re-coat 1
|
Friday, March 26, 2021, 13:55
Yesterday a heat shield was installed in the EVAP2.
A 1mm thick rhenium wire was held within two copper brackets to pass through a Cu tube with the intention of coating its inside face.
The desired temperature of the Re wire is 2500 degC
A water leak was performed and no leak was detected
|
Thursday, March 25, 2021, 11:24, Marla Cervantes, Empty, NA (Cu-Tube, , Done, Re-coat test 4
|
Objective: Coating the inner surface of a short tantalum tube with rhenium.
Result:
- The wire snnaped around 376 W (53 A, and 7.09 V) and 2170 °C (measured with filament pyrometer)
- The tube is coated
Thursday, March 25, 2021, 11:23
Yesterday a heat shield was installed in the EVAP2.
The desired temperature of the Re wire is 2500 degC
A water leak was performed (elog 539 describes it), no leak was detected.
Tuesday, March 23, 2021, 11:01
Pressure 3.8e-7 Torr, current rate set to 6 A @ 0.5 A/min
The wire started glowing at TGHT = 4W, 7A, 0.56V
When reaching 7A the current was increased 0.5 A manually
When reaching 16 A, the current was increased 1 A manually until reaching 54 A when the wire snapped |
Thursday, March 25, 2021, 07:57, Aaron Schmidt, , , , , Re - Ta test. Leak check.
|
Thursday, March 25, 2021, 07:55: Vacuum @ 5.12e-07T. Waterlines opened.
Thursday, March 25, 2021, 07:55: Vacuum @ 5.09e-07T. Stable.
|
Tuesday, March 23, 2021, 11:28, Marla Cervantes, Empty, 44489-6, , Done, Re-coating test 3
|
Objective: Coating the inner surface of a short tantalum boat with rhenium.
Result:
- The wire snnaped around 376 W (53 A, and 7.09 V) and 2170 °C (measured with filament pyrometer)
- The tube does not have indications of coating
Thursday, March 25, 2021, 11:23
Yesterday a heat shield was installed in the EVAP2.
The desired temperature of the Re wire is 2500 degC
A water leak was performed (elog 539 describes it), no leak was detected.
Tuesday, March 23, 2021, 11:01
Pressure 3.8e-7 Torr, current rate set to 6 A @ 0.5 A/min
The wire started glowing at TGHT = 4W, 7A, 0.56V
When reaching 7A the current was increased 0.5 A manually
When reaching 16 A, the current was increased 1 A manually until reaching 54 A when the wire snapped |
Tuesday, March 23, 2021, 08:07, Aaron Schmidt, , , , , Re - Ta test. Leak check.
|
Modified HS installed with new brackets as per Marla.
Tuesday, March 23, 2021, 08:02: Vacuum @ 3.64e-07T. Waterlines opened.
Tuesday, March 23, 2021, 08:06: Vacuum @ 3.60e-07T. Stable.
|
Tuesday, March 16, 2021, 08:29, Darwin Ortiz Rosales, TaC, , TARGET BOAT, Done, sintering of TaC on Caps and springs
|
Tuesday, March 16, 2021, 08:28
Each endcap is separated with a disc of graphite foil and rolled into packs of 5 within a foil envelope in a target boat.
There are also 4 coated springs, one in between endcaps and three on the ends
The boat is wrapped with 3-layers of Ta heatshields.
Chamber pumping down
OMEGA slope = 0.99
Will ramp TGHT up to 40 A then autoramp to 400A at 1A/min.
Final desired temperature on OMEGA (tap)= 1800C
Tuesday, March 16, 2021, 11:22
IGP1= 3.5e-06 Torr
TGHT = 40A, 0.4V
Will ramp up at 1A/min to 400 A
Wednesday, March 17, 2021, 08:06
IGP1= 2.98 e-07 Torr
TGHT = 400 A, 4.3V
OMEGA shows no temperature reading. Will ramp up to 450A at 1A/min
Wednesday, March 17, 2021, 08:58
OMEGA still shows no reading
IGP1= 4.2e-07 Torr
ramping to 470A @ 1A/min
Wednesday, March 17, 2021, 09:21
OMEGA no reading
IGP1 = 4.4 e-07 Torr
TGHT = 470 A, 5V
ramp up to 490 A at 1A/min
Wednesday, March 17, 2021, 11:05
TGHT at 490 A, 5.2 V since 10 am. Will start cooling at 2 pm.
Wednesday, March 17, 2021, 13:47
TGHT = 493A, 5.3V
IGP1= 3.2e-07 Torr and stable
Start ramp down at -2A/min
Thursday, March 18, 2021, 11:20
The boat was dismounted but the materials had not sintered properly. The boat looked very twisted. Everything was transferred to a new boat with uncoated Ta caps at either end.
It was left overnight to establish vacuum.
Friday, March 19, 2021, 08:23
IGP1= 2.2 e-07 Torr
initiate heating at 1A/min on TGHT to 60 A
Friday, March 19, 2021, 10:04
IGP1= 3.6 e-07 Torr
TGHT = 60 A, .73 V
Ramp up to 450 A @ 2A/min
Friday, March 19, 2021, 14:26
OMEGA 1895 at 455A, 8.4 V
manually ramp down to 1800C
OMEGA 1800C at 416A, 7.6V
will leave like that for 3 hours more
Friday, March 19, 2021, 17:12
OMEGA 1795 C
TGHT = 415A, 7.6V
IGP1= 6.8e-07 Torr
Start ramp down at -2A/min
Monday, March 22, 2021, 23:07
Marla removed from Evap 2. Sintering vwas very good. The container with Ta caps is better for sintering these pieces.
|
Tuesday, March 09, 2021, 11:54, Darwin Ortiz Rosales, TaC, 42464-1, HP-FEBIAD, Done, TaC coating/sintering
|
Tuesday, March 09, 2021, 11:54
Container coated with TaC and wrapped with 3 Ta heat shields.
Desired temperature= 1900 C, Omega Slope set = 0.990, Auto TGHT at 0.2A/min to reach 400A, TGHT will be increased accordingly to reach desired Temp.
TBHT will be set fixed at 230 A max).
Good vac at 3.00e -5 Torr
Bad vac at 5.00e-5 Torr
Chamber pump down
Wednesday, March 10, 2021, 08:32
IGP1 = 2.6 e -07 Torr
Start autoramp @ 1A/min to 40 A on both TGHT and TBHT
***Autoramp aborted due to work on EF12 affecting EVAP2***
Will have to resume Thursday or Friday
Saturday, March 13, 2021, 7:54
IGP1= 3.8e-07 Torr
Initiate heating @ 0.5A/min TBHT and TGHT to 60 A
Saturday, March 13, 2021, 23:01
IGP1 = 2.7e-07Torr
TGHT = 60.5A, 0.7V
TBHT= 60.0A, 0.7V
Initiate ramp @ 1 a/min to 400 A on TGHT and 230A on TBHT
Sunday, March 14, 2021, 08:45
IGP1= 8.2e-07 Torr
TGHT = 400A, 5.6V
TBHT = 232.9A, 3.0V
OMEGA = 1142 C
Continue ramping to 460 A on TGHT at 1a/min
Sunday, March 14, 2021, 10:11
IGP1 = 1.0 e-06 Torr
TGHT= 460.4 A, 6.5 V
TBHT = 232.9 A, 3.0 V
OMEGA = 1239 C
Will ramp up to 500 A at 1a/min on TGHT
Sunday, March 14, 2021, 10:53
IGP1 = 1.3 e-06 Torr
TGHT= 495 A, 7.2 V
TBHT = 232.9 A, 3.0 V
OMEGA = 1316 C
Will ramp up to 600 A at 1a/min on TGHT
Sunday, March 14, 2021, 12:45
IGP1 = 3.0 e-06 Torr
TGHT= 604 A, 9.1 V
TBHT = 232.9 A, 3.1 V
OMEGA = 1610 C
Will ramp up to 660 A at 1a/min on TGHT
Sunday, March 14, 2021, 17:01
IGP1= 2.4e-06 Torr
TGHT = 664 A, 10V
TBHT = 232.9 A, 3.1V
OMEGA = 1733 C
tapping TGHT to 740 A
OMEGA = 1883 C
Sunday, March 14, 2021, 21:45
IGP1= 3.1e-06 Torr
TGHT = 744A, 11.5V
TBHT = 232.9 A, 3.2V
OMEGA = 1875 C
Start cooling TGHT @-3A/min and TBHT @-1A/min
|
Friday, March 05, 2021, 10:48, Darwin Ortiz Rosales, TaC, 44691-1, LP-SIS, Done, TaC coating/sintering
|
Friday, March 05, 2021, 10:47
Ta tube was coated with TaC and wrapped with Ta heat-shields (3 layers)
Initial weight including heat-shields = 431.0 g
Desired temperature = 1900 C (expected TGHT ~430 A), TBHT will be set fixed at 230A (max).
Evap 2 will be pumped down over night.
Good vacuum = 3.00 e-5 Torr
Bad vacuum = 5.00 e-5 Torr
Saturday, March 06, 2021, 10:29
IGP1= 2.7 e-07 Torr and stable
AutoRamp at 1A/min to 40 A on TGHT and TBHT
Saturday, March 06, 2021, 22:36
IGP1= 2.2e-07 Torr
TGHT = 40.3 A, .46V
TBHT = 38.48 A, .48 V (set to 40 A)
Start Autoramp at 0.5A/min to 400 A on TGHT and 230A on TBHT
Sunday, March 07, 2021, 07:48
IGP1=8.5e-7 Torr
TGHT = 287 A, 4.6V
TBHT = 232 A, 4.0 V
OMEGA = 1493C
Increase ramp speed on TGHT to 2A/min to 400A
Sunday, March 07, 2021, 08:36
IGP1=1.7 e-06 Torr
TGHT = 373.7 A, 6.3V
TBHT = 232.9 A, 4.1 V
OMEGA = 1752 C
Sunday, March 07, 2021, 08:53
IGP1= 1.7e-06 Torr
TGHT = 400 A, 6.8 V
TBHT = 232.8 A, 4.1 V
OMEGA= 1842
Ramp TGHT @ 2A/min to 420 A as per attached current approximation
Sunday, March 07, 2021, 09:25
OMEGA=1915 C
TGHT = 420A, 7.2V
TBHT= 232.8 A, 4.1V
IGP1= 1.6 e-06 Torr
Tap down manually to approx 1900 C
TGHT = 412.9 A, 7.0 V and OMEGA=1900 C
Will leave for about 4 hours at this temperature
Sunday, March 07, 2021, 13:05
IGP1= 1.1 e-06 Torr
TGHT = 415 A, 7.2 V
TBHT = 232.8 A, 4.1 V
OMEGA = 1880C
Start cool down at -2A/min on TGHT and -1A/min TBHT
|
Tuesday, March 02, 2021, 11:32, Darwin Ortiz Rosales, TaC, 44691-5, LP-SIS, Done, TaC coating/sintering
|
Tuesday, March 02, 2021, 11:26
Ta tube was coated with TaC and wrapped with Ta heat-shields (3 layers)
Initial weight including heat-shields = 433.8 g
Desired temperature = 1900 C (expected TGHT ~430 A), TBHT will be set fixed at 230A (max).
Evap 2 will be pumped down over night.
Good vacuum = 3.00 e-5 Torr
Bad vacuum = 5.00 e-5 Torr
Wednesday, March 03, 2021, 13:28
IGP1 = 4.0 e-7 Torr
Start ramping @ 1A/min to 20A on both TGHT and TBHT
Wednesday, March 03, 2021, 15:03
Start ramping @1/min to 60A on Both TGHT and TBHT
Wednesday, March 03, 2021, 22:42
TGHT = 60A, TBHT = 60A
IGP1= 4.2 e-7 stable
Start ramping to 400A @ .5A/min for TGHT and @0.5A/min for TBHT to 230A
Thursday, March 04, 2021, 11:56
TGHT = 400 A, TBHT =230A
IGP1= 1.9e-6 Torr
OMEGA = 1695 C
Continue ramp up @0.5A/min to 430A on TGHT
Thursday, March 04, 2021, 14:02
IGP1 = 1.87e-6 Torr
TGHT = 434 A , 7.2 V
OMEGA = 1787 C
Will tap up manually 450A @ on TGHT and leave at that current for ~4 hours
Thursday, March 04, 2021, 19:35
After ~ 5 hours at 1829 C max OMEGA reading
OMEGA = 815 C
Start ramp down at 1A/min on TGHT and 0.8A/min for TBHT
IGP1= 1.2e-6 Torr
|
Monday, March 01, 2021, 13:58, Aaron Schmidt, , , , , Flex - line HS installed
|
Flex-Line HS had been fully scrubbed out earlier. All gaskets replaced.
Empty. Quick check for leaks.
Monday, March 01, 2021, 13:57: Roughing.
Monday, March 01, 2021, 14:13: TP1 on.
Monday, March 01, 2021, 15:18: Vacuum @ 1.01e-05T. Open HS waterline.
Monday, March 01, 2021, 15:24: Vacuum @ 9.30e-06T & dropping. Waterline ok.
Monday, March 01, 2021, 15:25: Turbo pump off. Vent when ready. |
Friday, February 26, 2021, 09:28, Ferran Boix Pamies, Empty, none, , Done, Parasitic target thermal tests
|
Tests were performed with external power supply. No target boat or container.
Small power on heating small heating elements on parasitic target attached on isac heatshield with water cooling on.
|
Tuesday, February 23, 2021, 08:59, Marla Cervantes, , NA (Cu-tube), , Done, Re coating Test 2
|
Tuesday, February 23, 2021, 08:49
Yesterday a heat shield was washed and when dry it was installed in the EVAP2,
A 1mm thick rhenium wire was held within two copper brackets to pass through a Cu tube with the intention of coating its inside face
Tuesday, February 23, 2021, 08:58 IGP1 = 7.7e-7 Torr
Pressure 5.88e-7 Torr, current rate set to 10 A @ 0.5 A/min
Pressure 6.1e-7 Torr, current rate set to 20 A @ 0.5 A/min
Pressure 8.51e-7 Torr current rate set to 30 A @ 0.5 A/min, temperature corrected 1800 degC (measured with filament pyrometer)
After 10 min the current and voltage are stable and the pressure is going down
Tuesday, February 23, 2021, 16:25
It seems like the wire is touching the tube so the system will be cool down.
Pressure 6.8e-7 Torr current rate set to 0A at -0.1 A/min
Tuesday, February 23, 2021, 17:38
Pressure 6e-7 Torr, TGHT = 23.3 A, 4.854 V, Temp 1788 deg C Omega, 1540 degC filament
current rate set to 0A at 0.2A/min
Wednesday, February 24, 2021, 09:37
Venting EVAP2
Wednesday, February 24, 2021, 16:47
The wire and Cu tube were fix such that the wire's deformation does not lead it to touch the tube, then the assembly was attached again and the EVAP2 was pumped down.
IGP1 = 9.3e-7 Torr, current rate is set to 5 A at 0.5 A/min
Wednesday, February 24, 2021, 17:04
IGP1 = 9e-7 Torr TGHT = 5.175A, 0,749 V
current rate is set to 10 A at 0.5 A/min
Wednesday, February 24, 2021, 17:23
IGP1 = 8.8e-7 Torr, TGHT = 10A, 1.78V
current rate is set to 20 A at 0.5 A/min
Since the wire seemed to be touching the tube, the system was vented.
The tube was shifted and the heat shield installed again, the system was pumped over nigth.
Thursday, February 25, 2021, 09:15
A water leak was performed and no leak was observed
IGP1= 4.95e-7 Torr
Thursday, February 25, 2021, 09:32 The current is increased at 0.5 A/min to 5 A
Thursday, February 25, 2021, 10:00
The current was tapped manually at 0.5 A to 6 A the wire is now glowing dimmly
Current rate set to 10A at .5 A/min
Current rate set to 20 A at 0.5A/min
Current rate set to 30 A at 0.5A/min
Thursday, February 25, 2021, 11:17 IGP1= 5.7e-7 Torr, TGHT=30.5A, 6.718V, filament=1740 degC
voltage and current stable, pressure going down.
Thursday, February 25, 2021, 11:21
Current rate set to 40 A at 0.4 A/min
Thursday, February 25, 2021, 11:53 IGP1 = 5.9e-7 Torr, TGHT = 9.267V, 39.15A, filament = 2060 degC
voltage and current stable, pressure going down.
Current rate set to 50 A @ 0.2A/min
During ramping the voltage reduced a bit and I decided to stop the ramp and reduce the current, the voltage stayed constant but the current started increasing slowly without me inputting it so I decided to ramp down the current at 0.2A/min.
When the current reached 0A the power supplies and the pumps were turned off, after an ~1h when the turbo pump had already stopped, the EVAP2 was vented and open.
The wire sintered to the copper tube confirming that the wire was in contact with the tube during heating.
The Cu tube present a grey metallic coloration indicating a Re coating.
The set up together with the copper heat shield were removed from the |
Saturday, February 13, 2021, 08:14, Darwin Ortiz Rosales, SiC, 41992-1, TARGET BOAT, Done, Sintering of SiC discs for SEM
|
Saturday, February 13, 2021, 08:10
Ta boat loaded with 80 discs enclosed in graphite foil in pockets of 20. Sample A at both ends and sample B in the middle spaced out. Boat wrapped in Ta heat-shields (3 layers).
(A B B A)
Desired temperature= 1800C (expected TGHT approx 410 A).
good vacuum = 3.00 e-05 Torr
bad vacuum = 5.00 e-05 Torr
Evap2 left to pump down over previous night.
IGP1= 5.4e-7 Torr and stable
Initiating TGHT ramp up at 1 A/ min to 30 A
Saturday, February 13, 2021, 12:19
IGP1= 6.9e-06 Torr
Ramp to 50 A 1A/min
Saturday, February 13, 2021, 14:35
IGP1 = 6.4e-6 Torr
Pressure trending down.
Saturday, February 13, 2021, 14:56
IGP1= 4.9 e-6 Torr
Initiate Ramp up @ 1 A/min to 400 A
Changed ramp up to 0.5 A/min at around 11:30 pm
Sunday, February 14, 2021, 11:43
The current will be ramped up to 420 A according to the trendline approximation (see attachement 1)
Sunday, February 14, 2021, 12:26
IGP1 = 8.9 e-06 Torr and trending down
TGHT = 420 A, 7.5 V
OMEGA = 1730 C
Will ramp up to 428 A manually
Sunday, February 14, 2021, 12:30
Reached 428 A on TGHT.
OMEGA = 1760 C
Will bump to 430 A and hold for 4 hours
OMEGA= 1765 C
Sunday, February 14, 2021, 18:00
OMEGA = 1789 C
IGP1= 7.5 e -7 Torr
TGHT = 430.5 A , 7.8 V
Start ramping down at -1A/min to zero A
|
Thursday, February 11, 2021, 10:57, Marla Cervantes, , NA, , Done, Re coating Test 1
|
Thursday, February 10, 2021, 12:00
Objective: Heat a Re wire to evaporate it and deposit a layer of Re on the inner surface of a Ta tube.
A Re wire of 1mm diameter was clamped with Cu brackets in EVAP2, the wire is partially enclosed in a Ta tube. EVAP2 pumping down
The wire needs to be heated to 2500 degC since this is its sublimation temperature at 8e-7 Torr
There is not a reliable system to measure the temperature of the wire but the readings of the micron, manual, and omega pyrometers will be register.
According to COMSOL simulations a power and taking in consideration the EVAP2's power loss, a power of 520 W (5A, 10V) is required.
Thursday, February 11, 2021, 15:39
Pressure 3.78e-7 Torr, current rate set to 10 A @ 0.5 A/min
Thursday, February 11, 2021, 16:32
Pressure: 4.01e-7 Torr, TGHT = 10A, 1.719 V. The voltage has stabilized, the wire is glowing but not enough for reading with micron nor omega, manual reads 970 degC. Also, the wire formed an arc (crest).
Thursday, February 11, 2021, 16:44
Pressure 3.8e-7 Torr, TGHT = 10 A, 1.723 V ramp set to 20A @ 0.2 A/min
Thursday, February 11, 2021, 17:26
Pressure increasing 4.7e-7 torr, TGHT = 20 A, 4.016 V, the wire does not seem to be changing,
Thursday, February 11, 2021, 18:02
Ramp set to 30A @0.4A/min
Pressure 7.2e-7 Torr, TGHT = 30A, 6.561V, manual pyrometer reads 1720degC
Ramp set to 40A @0.4A/min
Thursday, February 11, 2021, 18:35
Pressure 2.1e-6Torr and increasing, TGHT = 40A, 9.1V, manual pyrometer reads ~1880 degC
Ramp set to 50A @ 0.4 A/min
|
Tuesday, February 09, 2021, 06:48, Aaron Schmidt, , NA, , Done, Ta coating test
|
Monday, February 08, 2021, 17:00: Installed brackets w/ Ta wire and a small piece of Re to test voltage drop.
Rough down, TP on. Waterlines open.
Tuesday, February 09, 2021, 06:44: Vacuum @ 8.63e-07T.
Tuesday, February 09, 2021, 06:45: Shut TP & roughing pump ff. Valves are close. Ready for power outage.
Tuesday, February 09, 2021, 11:30: BP1 & TP1 back on.
Tuesday, February 09, 2021, 11:37: PS on. Vacuum @ 9.7e-06T & continuing down.
micron slope 0.98
Tuesday, February 09, 2021, 16:01 Pressure 7.26e-7 Torr
aiming at a temperature of 2000 degC on the wire; wire is not in the visual range of pycnometer; simulations of the system indicate that wire will be at 2000 degC at 60 W, hence current will be increased slowly.
Rate: 0.1 A/60 s to 10 A
Tuesday, February 09, 2021, 16:47 Tendence showed that at 5 A the power will be ~10 W, final ramping step was updated accordingly.
Tuesday, February 09, 2021, 16:49 Pressure dropping a bit: Current reading 7e-7 Torr
Tuesday, February 09, 2021, 17:09Pressure going down, curent will be ramped down at 0.2 A/min
Pressure: 6.958e-7 Torr, TGHT: 5 A, 2.748 V, omega is reading 1625 degC somewhere somehow, wire will stay at this conditions for 10 min to see if there is a pressure or voltage change.
Tuesday, February 09, 2021, 17:16 voltage and temperature are slowly increasing 2.789 V, and 1688 degC respectively.
Tuesday, February 09, 2021, 17:32 Voltage signal is noisy but it seems like the voltage is not increasing anymore, preassure has remained constant, wire is glowing, 1100 degC with manual pyrometer.
Tuesday, February 09, 2021, 17:44 TGHT: 2.81 V, 4.95 A, IGP1 6.63e-7 Torr. current will be increased manually at 0.2 A steps. At first step voltage is stable.
Tuesday, February 09, 2021, 18:13 TGHT: 6.6A, 3.981V (~26W), Omega 1741 degC and manual pyrometer ~1300 degC
Tuesday, February 09, 2021, 18:28 TGHT: 8A, 5.121V (~40W), omega 1816 degc, 1390 degC with manual pyrometer, step changed to 0.4A.
Tuesday, February 09, 2021, 18:34 TGHT: 8.8A, 5.88V (50W), omega 2008 degC, 1500 manual pyrometer
Tuesday, February 09, 2021, 18:56 TGHT: 9.6A, 6.64V, manual pyrometer 1800 degC, omega 2042 degC, wire is shinny enough for micron 2092 degC.
Tuesday, February 09, 2021, 19:01TGHT: 10A, 7V, ~1800 degC manual pyrometer, omega 2123 degC, micron 2152 degC
Tuesday, February 09, 2021, 19:15 TGHT: 10.5A, 7.47V, 2150 degC Omega, 2165 degC, ~1800 degC manual
Tuesday, February 09, 2021, 19:23 TGHT: 11A, 7.93 V, 2188 omega, 2210 deC micron
Tuesday, February 09, 2021, 19:29 TGHT: 11.5A, 8.37V, 2188 omega, 2210 deC micron
Tuesday, February 09, 2021, 19:33 TGHT: 12A, 9V, 2325 degC, 1900 degC manual, the wire changed shape and the preassure increase a bit , micron was readjusted to read, micron 2454 degC. Wire might be touching tube, only one more amper will be imputed.
Tuesday, February 09, 2021, 19:55 TGHT 13A, 9.865 V, 2404 degC omega , 2558 degC micron, manual pyrometer still reads 1800 degC, pressure increased with the power increment, bbut it seems like the wire touching the tube so no more current will be imputed.
Tuesday, February 09, 2021, 20:08 started ramping at -0.2A/min
Wednesday, February 10th , 20211, 10:00 System unloaded from EVAP2, wire has straightened, it has not sintered to the copper brackets, system is clean there is no evidence of coating. |
Monday, February 01, 2021, 13:57, Darwin Ortiz Rosales, SiC, 40282-4, TARGET BOAT, Done, Sintering of SiC discs for SEM
|
Monday, February 01, 2021, 13:52
Ta boat loaded with 20 Disc on either end capped with Ta springs to prevent overexpansion. discs wrapped Graphite foil and boat wrapped in Ta heat-shields (3 layers).
Sample A on left side and sample B on right side.
Desired temperature= 1800C (expected TGHT 410 A).
good vacuum = 3.00 e-05 Torr
bad vacuum = 5.00 e-05 Torr
Evap2 left to pump down over night.
Tuesday, February 02, 2021, 10:01
Pressure stable at IGP1= 7.8e-7 Torr
TGHT autoramp set to 50 A @ 1/min
Tuesday, February 02, 2021, 13:45
IGP1=3.5e-6 Torr
TGHT =49.9 A, 0.56 V
Ramp at 1A/min to 100A
Wednesday, February 03, 2021, 08:25
IGP1= 5.5 e-07 Torr
TGHT = 100 A, , 1.2 V
Yesterday the camera failed to operate. Cloud service discontinued. The TS camera is offline but it is a different provider. Will start ramping to 400A .
Ramp rate 2A/min
Wednesday, February 03, 2021, 15:55
ramped up to 520 A and 9.1V TGHT
Temperature average 1644 C but suspect actual temperature higher.
Held for 5 hours and started ramp down at -2A/min
Thursday, February 04, 2021, 9:35
IGP1= 2.99e-7 Torr
Begin pumpdown procedure and remove container
Note: SiC evaporation on most discs. The temperature was too high. Need to repeat.
|
Tuesday, November 24, 2020, 12:56, Marla Cervantes, , 44139-8-SK , TARGET BOAT, Done, Graphite casting conditioning
|
Tuesday, November 24, 2020, 09:23
A batch of 60 discs of 18 mm diameter were loaded in a tantalum tube. The tantalum tube was wrapped with 3 layers of Ta foil for heat shielding and mounted in the EVAP2. EVAP2 pumped down overnight and Aaron made a leak test this morning (elog 524).
The target material will be heated to 1990 degC. To measure the temperature, the tube has a Ta foil close to the graphite foils and it is held in place with a tantalum spring. Another Ta spring holds the graphite foils in the opposite side of the tube. The temperature will be measured with the Omega pyrometer (slope 0.99)
IGP1 = 6e-7 Torr. Note: The pressure has an usual behavior (see 2020-11-24-IGP1 and 2020-11-24IGP1-zoom out). After ~9 hrs, the pressure became stable (see 2020-11-24IGP1 -stable)
Tuesday, November 24, 2020, 13:00
IGP1 = 6.7e-7 Torr
Good vacuum of 3e-2 Torr and Bad vacuum 5e-2 Torr
The autoramp is set to 80 A at 1 A each 10 s
Tuesday, November 24, 2020, 13:43
IGP1 = 2.7e-5 Torr
TGHT = 1.13 V 80.5 A
Autoramp is set to to 100 A at 1 A each 20 s
Tuesday, November 24, 2020, 13:57
IGP1 = 2.5e-5 Torr and going down
TGHT = 100.2 A, 1.47 V
Autoramp is set to to 120 A at 1 A each 20 s
Tuesday, November 24, 2020, 14:06
IGP1 = 2.09e-5 Torr
TGHT = 1.6 v, 122 A
Autoramp is set to 200 A at 2 A each 10 s
Tuesday, November 24, 2020, 14:18 IGP1 = 5.4e-5 Torr
IGP1 = 1.5e-5 Torr
TGHT = 2.9 V, 200.5 A
Omega = 1123 °C
Autoramp is set to 450 A, conditions:
2 A each 10 s with a good vacuum of 3e-2 Torr and a bad vacuum 5e-2 Torr
Tuesday, November 24, 2020, 14:45
The autoramp was stopped at 424 A
TGHT = 421.65 A, 8.353 V
IGP1= 2.5e-5 Torr and going down
Omega 2020 degC
The TGHT current was reduced to 420 A (8.27 V) and the temperature reduced to 2007 degC
Tuesday, November 24, 2020, 21:03
IGP1 = 2.09e-6 Torr
TGHT = 7.899 V, 421.312 A
Temperature = 1870 degC
Autoramp is set to 0 A at 1 A/min |
Tuesday, November 24, 2020, 08:13, Aaron Schmidt, , , , , Flex - line HS installed
|
Monday, November 23, 2020, 17:01: Flex-line HS installed.
Tuesday, November 24, 2020, 08:03: Vacuum @ 9.55e-07T.
Tuesday, November 24, 2020, 08:08: Vacuum Ok
Tuesday, November 24, 2020, 08:09: Modify Controls dialogue on IEVAP2:IGP1:RDVAC
Max value from 0.1 to 0.0001 to better view curve on the strip tool and monitor for vacuum spikes.
Tuesday, November 24, 2020, 08:13: TGHT / TBHT PS on.
|
Thursday, November 05, 2020, 15:13, Ferran Boix Pamies, Empty, 41882-2, TARGET BOAT, Done, cleaning treatment.
|
2020-11-05 15:44 empty and naked boat in for heating up system and clean up. Turbo on.
2020-11-06 16:58 IGP1:4e-7T leak check ok. Ramping up target to 500A. 1A/10s.
2020-11-09 12:43 The target was left at 1500degC during the weekend.
2020-11-17 14:11 turbo pump off. Slow venting.
2020-11-18 09:18 Evap2 vented. Target removed. |
Wednesday, November 04, 2020, 17:31, Ferran Boix Pamies, Empty, 41882-2, TARGET BOAT, Done, Parasitic target graphite outgassing.
|
2020-11-04 17:31: target installed with boat containing graphite container for outgassing. Roughing pump on.
2020-11-04 17:49 turbo on, leaving it pumping over night.
2020-11-05 11:32 leak check ok. Ramping up target to 200A 2A/10s.
2020-11-05 11:53 IGP1:1.1e-6T . Ramping up target to 300A 1A/10s.
2020-11-05 11:53 IGP1:1.2e-6T . Pyrometer:1320degC. Ramping up target to 400A 1A/10s.
2020-11-05 11:53 IGP1:1.8e-6T . Pyrometer:1650degC. Ramping up target to 500A 1A/10s.
2020-11-05 12:57 IGP1:3.4e-6T . Pyrometer:1910degC. Ramping up target to 525A 1A/10s.
2020-11-05 13:02 IGP1:3.6e-6T . Pyrometer:1990degC. Leaving it hot for 1h.
2020-11-05 14:00 IGP1:2e-6T stable . Pyrometer:1990degC. cooling down 2A/10s.
|
Monday, November 02, 2020, 18:32, Ferran Boix Pamies, Empty, 44139-7-SK, TARGET BOAT, Done, HEA heat treatment
|
2020-11-02 6:32: roughing on
2020-11-02 7:21: Turbo on for a while, IGP1:1.8e-5T . water leak check ok.
2020-11-02 7:47: IGP1:1e-5T . Ramping up target heater to 200A, 1A/10s.
2020-11-02 7:47: TGHT at 275A, pyrometer at 1300degC. Leaving it hot for 24h.
2020-11-04 9:06: After 37h treatment, ramping down to 0A.2A/10s.
2020-11-04 9:46: target ramped down. Venting.
2020-11-04 17:30: Big amounts of outgassing non detected in GP1 coated some inner walls in evap2. The walls got cleaned with acetone. All as before now.
|
Tuesday, October 27, 2020, 10:25, Ferran Boix Pamies, Empty, 44139-7-SK, TARGET BOAT, Done, parasitic target commissioning
|
2020-10-27 10:24 setup introduced yesterday. Pumping over night IGP1: 5.7e-7T. Water leak check ok. Performing heating elements check.
2020-10-27 10:43 Heating elements check show low cooling. Ramping up target 1A/15s to 200A.
2020-10-27 11:54 all ok 200A, thermocouples show room temperature on cartridge and heat shield. Ramping up target 2A/10s to 300A.
2020-10-27 11:54 all ok 300A, thermocouples show 28/25degC. Ramping up target 2A/10s to 400A.
2020-10-27 11:54 all ok 400A, thermocouples show 36.5/29degC. Ramping up target 2A/10s to 500A.
2020-10-27 11:54 all ok 500A, thermocouples show 48.9/33degC. Ramping up target 2A/15s to 550A.
2020-10-27 12:43 all ok 550A, thermocouples show 55/34degC. Ramping up target 2A/15s to 600A.
2020-10-27 12:43 all ok 600A, thermocouples show 61.5/35.2degC. Ramping up target 2A/15s to 625A.
2020-10-27 13:14 all ok 625A, thermocouples show 64.6/34.2degC. Ramping up target 2A/15s to 650A. |
Wednesday, October 21, 2020, 14:39, Aaron Schmidt, Nb, 44508-2, LP-SIS, In progress, Conditioning Nb#9
|
Nb#9 LP-SIS target description:
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.025mm
Target density = 7.24 g/cm3
Target length = 3.5 cm
Total Mass = 25.343 g [Incl foils + Ta wire on 6 packs]
Total mass w/ Target oven= 425 g (w/ end caps)
Discs in target are arranged as follows: 1pack / 75 singles / 1pack / 100 singles / 2packs / 100 singles / 1pack / 75 singles / 1pack
End caps installed (not yet expanded). No Ta foil heat shield added.
Final desired temperature = 1900C.
OMEGA slope = 0.98.
Wednesday, October 21, 2020, 14:09: Roughing.
Wednesday, October 21, 2020, 14:32: Turbo pump on.
Wednesday, October 21, 2020, 15:29: Waterlines opened. Vacuum ok @ 1.05E-05T.
Wednesday, October 21, 2020, 15:30: TGHT / TBHT PS on. Slope Set.
Wednesday, October 21, 2020, 19:06: Auto-ramping TGHT / TBHT to 300 / 100 @ 1 A per min. Vacuum @ 1.85e-06T.
Thursday, October 22, 2020, 07:26: Auto-ramping TGHT / TBHT to 500 / 200 @ 2 A per min. Vacuum @ 7.61e-07T.
Thursday, October 22, 2020, 11:28: Auto-ramping TGHT / TBHT to 580 / 230 @ 2 A per min. Vacuum @ 1.53e-06T. The Omega IR2C is back. Temp @ 1576 deg C.
Thursday, October 22, 2020, 12:22: Auto-ramping TGHT to 625 A @ 2 A per min. Vacuum @ 2.47e-06T. Temp @ 1734 C.
Thursday, October 22, 2020, 12:48: Auto-ramping TGHT to 645 A @ 2 A per min. Vacuum @ 3.11e-06T. Temp @ 1815 C.
Thursday, October 22, 2020, 13:10: Auto-ramping TGHT to 660 A @ 2 A per min. Vacuum @ 3.39e-06T. Temp @ 1851 C.
Thursday, October 22, 2020, 13:25: Manually tap up TGHT until 1900 C. Vacuum @ 3.53e-06T.
Thursday, October 22, 2020, 13:30: TGHT @ 673 A. Temp @ 1903 C. Vacuum @ 3.79e-06T.
Thursday, October 22, 2020, 14:00: Auto-cooling @ 1 A per min.
Friday, October 23, 2020, 07:50: PS off. Turbo pump off. Purge waterline.
Friday, October 23, 2020, 09:02: Venting. |
Friday, October 16, 2020, 16:31, Luca Egoriti, Empty, , TARGET BOAT, In progress, HPOG annealing
|
Friday, October 16, 2020, 11:30
Target mounted in EVAP2. Pump down started
Friday, October 16, 2020, 12:05
Pressure goes up. Checked with Ferran and he says that the valve IEVAP2:RV1 automatically closes sometimes. WEIRD, to be chacked.
Friday, October 16, 2020, 15:20
IGP2 bottoms at 0.2T, and doesn't increase recover if I close RV1 while it shouldn't (as shown before). --> Vented to restart from scratch
Friday, October 16, 2020, 15:45
Pumped down again, vacuum went down to 0.16 and then started raising until ~0.18. This time the valve was open indeed! opening and closing the valve had no effect on the vacuum as if the booster pump was not effective
Friday, October 16, 2020, 16:27
Tried a THIRD time, this time effectively, to turn the turbo ON. I managed to, but the turbo makes weird spinning sounds every ~30 sec. Moreover, its pumping down plot seems quite weird - see spike UP while pumping. Could it be related to a dysfunction of the backing pump?
|
Thursday, October 15, 2020, 18:51, Ferran Boix Pamies, Empty, 44139-7-SK, TARGET BOAT, Done, heat gun plus parasitic target thermal comissioning.
|
2020-10-15 18:51 : Setup installed during the day. Pumped down to IGP1:1.5e-5T , water leak check ok. Ramping up to 100A.
2020-10-15 19:30 : A heating element was showing bad signs and failed very early. ramping down and venting. |
Tuesday, October 13, 2020, 11:15, Ferran Boix Pamies, Empty, 44139-7-SK, TARGET BOAT, Done, foil heating
|
2020-10-13 11:13 Target was left under vacuum over the weekend. IGP1: 1.6e-7T water on- leak check ok. Ramping up 2A/30s to 100A.
2020-10-13 11:47 All ok at 100A. Ramping up, 1A/10s to 200A.
2020-10-13 12:08 All ok at 200A. Temp tc on foil 200degC. Ramping up, 1A/10s to 300A.
2020-10-13 12:08 All ok at 300A. Temp tc on foil 340degC. Ramping up, 1A/10s to 400A.
2020-10-13 12:48 All ok at 400A. Temp tc on foil 474degC. pyro shows 1050degC Ramping up, 1A/10s to 500A.
2020-10-13 13:06 All ok at 500A. Temp tc on foil 615degC. pyro shows 1238degC Ramping down, 1A/10s to 0A.
2020-10-13 17:04 The foil has been replaced due to suspected radiation transparency being the cause of low measured temperatures. A graphite and tantalum pack is now attached. Vacuum is back to IGP1: 9.5e-6T. Ramping up to 100A, 1A/10s.
2020-10-13 17:31 All ok at 100A. Temp tc on foil 80degC. Ramping up, 1A/10s to 200A.
2020-10-13 17:31 All ok at 200A. Temp tc on foil 310degC. Ramping up, 1A/10s to 300A.
2020-10-13 17:31 All ok at 300A. Temp tc on foil 468degC. Ramping up, 1A/10s to 400A.
2020-10-13 17:31 All ok at 400A. Temp tc on foil 598degC. Ramping up, 1A/10s to 500A.
2020-10-13 17:31 All ok at 500A. Temp tc on foil 700degC. Ramping up, 1A/10s to 600A.
2020-10-13 17:31 All ok at 600A. Temp tc on foil 760degC. Ramping down, 1A/20s to 0A.
2020-10-14 17:09 foils for radiation focusing have been replaced and doubled to reduce transmission. IGP1:1.5e-5T , water leak check ok. Ramping up to 100A 1A/10s.
2020-10-14 17:30 All ok at 100A. Temp tc on foil 60degC. Ramping up, 1A/10s to 500A.
2020-10-14 17:50 All ok at 200A. Temp tc on foil 378degC.
2020-10-14 18:10 All ok at 300A. Temp tc on foil 550degC.
2020-10-14 18:10 All ok at 400A. Temp tc on foil 705degC.
2020-10-14 18:10 All ok at 500A. Temp tc on foil 816degC.Ramping up, 1A/10s to 600A.
2020-10-14 18:10 All ok at 600A. Temp tc on foil 906degC.Ramping up, 1A/10s to 625A.
2020-10-14 18:10 All ok at 625A, IGP1: 1.3e-5T. Temp tc on foil 924degC.Ramping up, 1A/10s to 650A.
2020-10-14 19:21 All ok at 650A. Temp tc on foil 940degC.Ramping down, 1A/10s to 0A. Pyrometer on foil 1200degC
|
Friday, October 09, 2020, 09:50, Ferran Boix Pamies, Empty, 44139-7-SK, TARGET BOAT, Done, Tests, radiation gun for parasitic target
|
2020-10-09 9:48 The target was installed the day before and left pumping over night. IGP1=4.7e-7Torr. leak check when water on, ok. Setting ramp up
2020-10-09 10:16 Ramping up the target to 50A, 1.5A/30s. All good. Going to 200A same rate.
2020-10-09 11:11 Target at 200A. Pyrometer 1170degC. ramping to 300A same rate.
2020-10-09 11:51 Target at 300A. Pyr. 1510. Ramping to 400A same rate.
2020-10-09 12:27 Target at 400A. Pyr. 1820. Ramping to 500A same rate.
2020-10-09 13:01 Target at 500A. Pyr. 2100. Ramping down to 0A 2A/30s. |
Wednesday, October 07, 2020, 12:25, Aaron Schmidt, , , , In progress, IEVAP2:TP1 Swap out.
|
Wednesday, October 07, 2020
TP1 was not spinning up past 4krpm. Stalling & tripping out. Examined with Vacuum group, appears to be starting to seize. Exchange turbo pump.
Serial# 500937
Wednesday, October 07, 2020, 12:25: TP1 Exchanged.
Wednesday, October 07, 2020, 12:38: Roughing.
Wednesday, October 07, 2020, 13:55: Soft start initiated. Steps up krpm every 5 min. 10 steps.
Wednesday, October 07, 2020, 13:22 @ 24 krpm.
Wednesday, October 07, 2020, 13:42: TP1 at speed. 38 krpm.
Wednesday, October 07, 2020, 13:45: TP1 off. Soft start function off. Remote start configuration initiated. TP1 on. OK. |
Tuesday, October 06, 2020, 14:23, Aaron Schmidt, Ta, 44508-1, LP-SIS, In progress, Conditioning Ta#61
|
Ta#61 LP-SIS target description:
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.025mm
Target density = 12.76 g/cm3
Target length = 3.4 cm
Total Mass = 43.388 g [Incl foils + Ta wire on 6 packs]
Total mass w/ Target oven= 464 g (w/ end caps)
Discs in target are arranged as follows: 1pack / 100 singles / 1pack / 75 singles / 2packs / 75 singles / 1pack / 100 singles / 1pack
End caps installed (not yet expanded). No Ta foil heat shield added
TBHT will be ramped up to 230A at 1.0A/min.
TGHT will be ramped up to 600A + at 2.0A/min.
Final desired temperature = 1900C.
OMEGA slope = 0.98.
Tuesday, October 06, 2020, 14:17: Roughing.
Tuesday, October 06, 2020, 14:36: Turbo pump on.
Tuesday, October 06, 2020, 14:43: Turbo pump not spinning up. Holding at 4 krpm. Will need to vent and Troubleshoot in the am.
Attempted to run the turbo pump again. Only runs to 4 krpm. Shut down to avoid trip. Vent & remove Flex-line HS. Change all the SS gaskets. Re-install Flex-line HS w/ Ta#61.
Wednesday, October 07, 2020, 09:16: Roughing.
Wednesday, October 07, 2020, 09:32: Turbo pump on.
Wednesday, October 07, 2020, 10:05: Multiple attempts made to spin up the turbo pump. TP1 holds at 4 krpm, occasionally to 5 krpm, times out & trips.
Wednesday, October 07, 2020, 10:08: Shut off TP1 & backing pump.
Replaced TP1. https://elog.triumf.ca/TIS/Evaporator_2/514
Wednesday, October 07, 2020, 13:45: TP1 off. Soft start function off. Remote start configuration initiated. TP1 on @ 38krpm. OK.
Wednesday, October 07, 2020, 13:47: Vacuum @ 1.31e-05T.
Wednesday, October 07, 2020, 13:49: Waterlines opened. Vacuum ok @ 1.27e-05T.
Wednesday, October 07, 2020, 13:50: PS switched on.
Wednesday, October 07, 2020, 15:24: Slope set @ 0.98. Vacuum @ 3.30e-06T.
Wednesday, October 07, 2020, 15:26: TGHT / TBHT on. Manually tap up to 10 / 10 A.
Wednesday, October 07, 2020, 15:28: Auto-ramping TGHT / TBHT to 300 / 150 A @ 2 / 1 A per min.
Thursday, October 08, 2020, 05:23: Vacuum @ 7.00e-07T.
Thursday, October 08, 2020, 05:25: Auto-ramping TGHT / TBHT to 450 / 200 A @ 2 / 1 A per min. Temp @ 996 C
Thursday, October 08, 2020, 06:44: Auto-ramping TGHT / TBHT to 550 / 230 A @ 2 / 1 A per min. Temp @ 1426 C
Thursday, October 08, 2020, 07:43: Vacuum @ 3.88e-06T. Temp @ 1685 C.
Thursday, October 08, 2020, 07:45: Auto-ramping TGHT to 600 A @ 2 A per min.
Thursday, October 08, 2020, 08:42: Auto-ramping TGHT to 630 A @ 2 A per min. Vacuum @ 4.01e-06T. Temp @ 1800 C.
Thursday, October 08, 2020, 09:07: Auto-ramping TGHT to 645 A @ 2 A per min. Vacuum @ 4.91e-06T. Temp @ 1851 C.
Thursday, October 08, 2020, 09:19: Auto-ramping TGHT to 655 A @ 2 A per min. Vacuum @ 5.37e-06T. Temp @ 1879 C.
Thursday, October 08, 2020, 09:28: TGHT @ 650-657 A. Vacuum @ 5.70e-06T. Temp @ 1901 C. Desired temperature reached*
Thursday, October 08, 2020, 09:59: TGHT @ 650-657 A. Vacuum @ 4.64e-06T. Temp @ 1903 C.
Thursday, October 08, 2020, 10:01: Auto-cooling TGHT / TBHT @ -3 / -2 A per min.
Thursday, October 08, 2020, 13:57: TP1 / PS off.
Thursday, October 08, 2020, 14:08: Venting.
Thursday, October 08, 2020, 14:15: Flex-Line HS removed w/ Ta#61. |
Monday, September 28, 2020, 11:53, John Wong, np-SiC, , TARGET BOAT, In progress, np-SiC carbonization
|
Monday, September 28, 2020, 11:49
6 discs of np-SiC were loaded to the target boat wrapped with 3 layers of heat shields.
Desired temperature at 1500 C, (As per e-log 414/416, TGHT = 450A/7.31V, 3.28kW)
Omega slope set at 1.05 (for carbide)
Good vac = 3.0e-5 Torr,
Bad vac = 5.0e-5 Torr.
Pumping down in progress
Monday, September 28, 2020, 21:44
Pressure at 1e-6 Torr. Initiated autoramping at 0.2A/min to reach 300 A. Monitor temp.
Wednesday, September 30, 2020, 11:39
TGHT reached to 300 A/ 4.5V, temp at 1130 C. No coating on windows.
Continue to ramp up 330A. Monitor temp.
Wednesday, September 30, 2020, 16:38
TGHT reached 330 A / 5.04 V, temp at 1190 C.
Ramp up to 400 A. Current pressure at 9.8 e-7 Torr.
Thursday, October 01, 2020, 10:28
TGHT reached 400 A/ 6.3V, temp at 1320 C. Continue to ramp up to 450 A.
Thursday, October 01, 2020, 16:44
TGHT reached to 450 A/ 7.4 V. TEmp at 1500 C.
Pressure at 1.35 e-6 Torr and coming down. Continue to hold TGHT at 1500 C for at least 24 hr.
Sunday, October 04, 2020, 16:49
TGHT has been holding at 450 A/ 7.3 V for nearly 3 days; temp has gone up and stabilized at 1554 C; pressure at 2.13 e -7 Torr.
Initiated cooling down at -2A/min.
Monday, October 05, 2020, 10:02
Chamber vented.
|
Friday, September 25, 2020, 10:32, Darwin Ortiz Rosales, Nb, , TARGET BOAT, Done, Heat Treatment of Nb for Edward
|
Friday, September 25, 2020, 10:30
Target boat with a layer of niobium foil on the bottom is used to heat up Nb samples to 1400 C for 4 hrs.
OMEGA slope = 0.99
The niobium samples are wrapped in two layers of Nb foil.
Boat is wrapped with 2 layers of Ta foil, careful to avoid touching samples.
Friday, September 25, 2020, 10:35
Manually ramped TGHT to 40 A and kept at that current for approximately 15 minutes.
Then started autoramp at 1A/min up to 100 A
Friday, September 25, 2020, 16:58
IPG1= 4.7e-07 Torr
TGHT =100.0 A, 1.3 V
Start autoramp to TGHT to 300 A @ 2A/min
@ 300A temperature = 1179 C
Friday, September 25, 2020, 20:00
autoramp to 345 A
Friday, September 25, 2020, 20:39
TGHT = 345 A, 5.4 V
OMEGA = 1296 C
IPG1= 8.1 e-07 Torr
Ramp manually to 1400 C
Friday, September 25, 2020, 20:51
reached 1400 C on OMEGA at TGHT = 476 A
Friday, September 25, 2020, 20:59
OMEGA increased to 1410, lowered TGHT to 468 A to get back to 1400 C on OMEGA
Friday, September 25, 2020, 21:40
Lowered TGHT to 463 A, 5.79 V to bring OMEGA to 1400 C from 1404 C
Saturday, September 26, 2020, 00:51
Sample has been at 1400 C for 4 hours.
IGP1= 7.2 e-07 Torr
Cooling at- 2A/min
|
Monday, September 28, 2020, 09:36, John Wong, Nb, , TARGET BOAT, Done, Heat Treatment of Nb for Edward
|
Darwin Ortiz Rosales wrote: |
Friday, September 25, 2020, 10:30
Target boat with a layer of niobium foil on the bottom is used to heat up Nb samples to 1400 C for 4 hrs.
OMEGA slope = 0.99
The niobium samples are wrapped in two layers of Nb foil.
Boat is wrapped with 2 layers of Ta foil, careful to avoid touching samples.
Friday, September 25, 2020, 10:35
Manually ramped TGHT to 40 A and kept at that current for approximately 15 minutes.
Then started autoramp at 1A/min up to 100 A
Friday, September 25, 2020, 16:58
IPG1= 4.7e-07 Torr
TGHT =100.0 A, 1.3 V
Start autoramp to TGHT to 300 A @ 2A/min
@ 300A temperature = 1179 C
Friday, September 25, 2020, 20:00
autoramp to 345 A
Friday, September 25, 2020, 20:39
TGHT = 345 A, 5.4 V
OMEGA = 1296 C
IPG1= 8.1 e-07 Torr
Ramp manually to 1400 C
Friday, September 25, 2020, 20:51
reached 1400 C on OMEGA at TGHT = 476 A
Friday, September 25, 2020, 20:59
OMEGA increased to 1410, lowered TGHT to 468 A to get back to 1400 C on OMEGA
Friday, September 25, 2020, 21:40
Lowered TGHT to 463 A, 5.79 V to bring OMEGA to 1400 C from 1404 C
Saturday, September 26, 2020, 00:51
Sample has been at 1400 C for 4 hours.
IGP1= 7.2 e-07 Torr
Cooling at- 2A/min
|
Monday, September 28, 2020, 09:36
Vented chamber - for Darwin.
|
Thursday, September 24, 2020, 13:37, Aaron Schmidt, Nb, , TARGET BOAT, , Nb Test SRF group
|
Sample loaded into a vertical target boat. Flex line HS removed, SS waterline HS installed -AS.
Thursday, September 24, 2020, 13:22: Roughing.
Thursday, September 24, 2020, 13:54: Turbo pump on. |
Monday, September 21, 2020, 17:01, Marla Cervantes, , 44139-8-SK, TARGET BOAT, Done, Conditioning graphite target #3
|
Monday, September 21, 2020, 16:50
450 graphite foils coated with graphite slurry were loaded in a tantalum tube, the tantalum tube was wrapped with 3 Ta heat shields and installed in the EVAP, to measure the temperature, a pack of 4 Ta foils were inserted in each side of the tube.
System is currently pumping down.
Tuesday, September 22, 2020, 07:54
IGP1 = 2e-6 Torr
Good vacuum of 3e-2 Torr and Bad vacuum 5e-2 Torr
The autoramp is set to 50 A at 1 A each 10 s
Tuesday, September 22, 2020, 08:18
IGP1 = 3.7e-6 Torr
TGHT = .586 V, 50.06 A
Autoramp is set to 80 A same conditions.
Tuesday, September 22, 2020, 08:26
IGP1 = 0.0006 Torr
TGHT = .97 V 80.3 A
Autoramp is set to to 100 A at 1 A each 20 s
Tuesday, September 22, 2020, 08:45
IGP1 = 0.003 Torr
TGHT = 1.3 V, 100.5 A
Autoramp is set to 120 A at same conditions
Tuesday, September 22, 2020, 09:36
IGP1 = 0.0001 torr
TGHT = 1.6 v, 122 A
Autoramp is set to 200 A at 2 A each 10 s
Tuesday, September 22, 2020, 10:19
IGP1 = 5.4e-5 Torr
TGHT = 2.9 V, 200.5 A
Omega = 1123 °C
AP = 1164 °C
Autoramp is set to 450 A,conditions:
2 A each 10 s with a good vacuum of 3e-2 Torr and a bad vacuum 5e-2 Torr
Tuesday, September 22, 2020, 11:24
TGHT = 447.8 A, 7.4 V
IGP1 = 3.7e-5 Torr
Omega = 1750 °C
AP = 1720.4 °C
Autoramp set to 520 A at same conditions
Tuesday, September 22, 2020, 11:38
TGHT = 8.9 V, 525.8 A
IGP1 = 4.8e-5 Torr
Omega = 1914 °C
AP = 1835.6 °C
Autoramp set to 560 A at same conditions
Tuesday, September 22, 2020, 12:13
Omega 2038 °C
Tuesday, September 22, 2020, 12:14
Current manually reduced to 555 A
TGHT = 9.8 V, 560.8 A
IGP1 = 2.5e-5 Torr
Tuesday, September 22, 2020, 12:17
Omega = 2030 °C
Tuesday, September 22, 2020, 12:19
Current manually reduced to 550 A
TGHT = 9.8 V, 547.8 A
IGP1 = 2.3e-5 Torr
Tuesday, September 22, 2020, 12:27
Omega = 2027 °C
Tuesday, September 22, 2020, 12:27
Current manually reduced to 540 A
TGHT = 9.6 V, 541.6 A
IGP1 = 2e-5 Torr
Tuesday, September 22, 2020, 12:34
Voltage suddenly increased!
TGHT = 10.3 V, 533.8 A
IGP1 = 2.9e-5 Torr
Omega = 2129 °C
Current reduced manually to 520 A to compensate the voltage increment
Tuesday, September 22, 2020, 12:52
Another voltage increment
TGHT = 9.9 V, 519.75 A
IGP1 = 1.9 e-5 Torr
Omega 2108 °C
Current reduced manually to 500 A to compensate the voltage increment
Omega = 2070 °C
Tuesday, September 22, 2020, 13:05
TGHT = 9.4 V, 492.4 A
Omega = 2063 °C
Tuesday, September 22, 2020, 13:08
Another voltage increment! this time it was an spike
Tuesday, September 22, 2020, 16:13
After 5 hours
IGP1 = 6e-6 Torr
TGHT = 9.5 V, 488 A
Autoramp was set to 0 A at 2 A/min
Omega = 2044 °C
AP = 2003.7 °C
Wednesday, September 23, 2020, 16:18
EVAP2 vented with air, target removed. |
Thursday, September 17, 2020, 16:11, Marla Cervantes, Empty, 44139-9, LP-SIS, Done, TaC coating/sintering
|
Thursday, September 17, 2020, 16:10
An LP-SIS was wrapped with 3 Ta layers, and installed in the EVAP2
Desired temperature= 1900 C, Omega Slope = 0.990
Friday, September 18, 2020, 10:56
IGP1 = 4.4e-7 Torr
Leak check performed, no leak observed
Friday, September 18, 2020, 11:16
Power supplies on.
Good vac at 3.00e -5 Torr
Bad vac at 5.00e-5 Torr
Autoramp at 0.5A/min to 400A on TGHT and 230A on TBHT
Friday, September 18, 2020, 11:21
Autoramp paused because, TBHT is not ramping
Ramping manually current to 10 A in 0.5 A steps
Friday, September 18, 2020, 11:38
Restarted autoramp (Autoramp at 0.5A/min to 400A on TGHT and 230A on TBHT)
Friday, September 18, 2020, 22:50
IGP1 = 2.04e-6 Torr
TGHT = 5 V, 322.8 A
TBHT = 4 V, 233.1 A
Omega = 1459 °C
Autoramp changed to 0.2 A/min to 450 A
Saturday, September 19, 2020, 10:49
IGP1 = 8e-7 Torr
TGHT = 7.3 V, 449.1 A
TBHT = 4 V, 233.1 A
Omega = 1789 degC
Saturday, September 19, 2020, 13:25
IGP1 = 6.5 e-7 Torr
TGHT 7.2 V, 447.975 A
TBHT = 4.08 V, 233.09 A
Omega = 1785 °C
Saturday, September 19, 2020, 13:26
Starting ramp down at Commence cooling at -2 A/min for TGHT and -1 A/min for TBHT
Monday, September 21, 2020, 09:16
Turning off pumps
Monday, September 21, 2020, 16:47
EVAP2 was vented with air and the tantalum oven was removed, the coating seems sintered. |
Thursday, September 10, 2020, 07:53, Aaron Schmidt, Empty, 41790-8, LP-FEBIAD, Done, Fernando FEBIAD / Anode testing.
|
FEBIAD installed. Anode PS installed. ANODE connected!.
Leak check
Thursday, September 10, 2020, 07:46: Vacuum @ 6.30e-07T
Thursday, September 10, 2020, 07:47: HS Waterline open. Stable vacuum.
Thursday, September 10, 2020, 07:51: Auto-ramp TGHT / TBHT to 400 / 200 A @ 2 A per min.
FM
Thursday, September 10, 2020, 13:28: Pyrometer aligned. Current reading 1106.7 @ slope=0.9
Thursday, September 10, 2020, 13:46: Auto-ramp TGHT / TBHT to 580/ 250A @ 2 A per min.
Thursday, September 10, 2020, 13:47: Recording pyrometer data
Thursday, September 10, 2020, 15:33: Auto-ramp finished. Temperature=1568.0 @slope=0.9
Thursday, September 10, 2020, 15:35: Voltage power supply limited to 150 mA.
Thursday, September 10, 2020, 15:36: Voltage power supply is set to output. Nothing strange on the other PS.
Thursday, September 10, 2020, 15:42: Slowly increased the voltage to 150 V but nothing read. two times during the voltage sweep the current on the Ps showed 1mA. Nothing strangeon the vacumm or the other power supply voltages
Thursday, September 10, 2020, 15:45: Auto-rampup TBHT to 290 @ 2A/min
Thursday, September 10, 2020, 16:08: Voltage sweep
Thursday, September 10, 2020, 17:24: Auto-rampup to 300 @ 2A/min
Friday, September 11, 2020, 11:05: Auto-ramping to 290 @ -2A/min
Friday, September 11, 2020, 13:22: auto-ramping to 305 @ 2A/min
Friday, September 11, 2020, 14:10: The power supply is not reading current anymore. At 305 A I couldn't get any reading. I lowered the current to 290 A and the PS displays 0 mA even at 500 V, whereas before it showed 13 mA.
Vacuum looks normal not any sort of spike.
I will open the system to inspect the interior.
Friday, September 11, 2020, 14:15: Auto-cooling to 0 A TGHT/TBHT @-2A/min
Saturday, September 12, 2020, 10:52: Venting
Saturday, September 12, 2020, 14:00: Confirmed anode de-attached. I will spot welded again.
Saturday, September 12, 2020, 18:29: After many failures I aborted the spot welding. The anode ended up looking pretty bad.
Sunday, September 13, 2020, 19:06: Opened waterlines. Vacuum still decreasing.
Monday, September 14, 2020, 09:12: Vacuum @ 8.15e-7 T. and decreasing. I will start the ramping now.
Monday, September 14, 2020, 09:28: Auto-ramping to 400/200 A @ 4/min (1 A/15 s) .
No reading on the 2-color pyrometer channel. 1-color channels indicate around 1000C
Monday, September 14, 2020, 12:49: Recording temperature and vacuum. Auto-ramp TBHT to 210 @ 4A/min.
Monday, September 14, 2020, 12:57: Emissivity slope sweep. Only "under" is being shown
Monday, September 14, 2020, 12:58: Auto-ramp TBHT to 220 @ 4A/min.
Monday, September 14, 2020, 13:05: Emissivity slope sweep. Only "under" is being shown
Monday, September 14, 2020, 13:06: Auto-ramp TBHT to 240 @ 4A/min.
Monday, September 14, 2020, 13:17: Auto-ramp TBHT to 250 @ 4A/min.
Monday, September 14, 2020, 13:22: Emissivity slope sweep. Only "under" is being shown
Monday, September 14, 2020, 13:23: Auto-ramp TBHT to 260 @ 4A/min.
Monday, September 14, 2020, 13:27 : Emissivity slope sweep. Only "under" is being shown
Monday, September 14, 2020, 13:27 : Auto-ramp TBHT to 275 @ 4A/min.
Monday, September 14, 2020, 13:36: Emissivity slope sweep. Only "under" is being shown for the 2-color channel. 1-color channel displays around 1200 C. Maybe there is a different cutoff for the 2-color channel
Monday, September 14, 2020, 13:38: At 400V the PS reads back 1mA
Monday, September 14, 2020, 13:39 : Auto-ramp TBHT to 290 @ 4A/min.
Monday, September 14, 2020, 17:41: Roughing
Tuesday, September 15, 2020, 07:03: Vacuum stable at 4.65e-7T.
Tuesday, September 15, 2020, 07:03: Auto-ramp TGHT / TBHT to 400/ 200A @ 4 A per min.
Tuesday, September 15, 2020, 10:00: Auto-ramp TGHT to 500 @ 4 A per min.
Tuesday, September 15, 2020, 11:13: Auto-ramp TBHT to 250@ 4 A per min.
Tuesday, September 15, 2020, 15:44: There is a short inside the system. I thought it might be the vanadium wire but increasing the tbht current did not indicate a clear evaporation so I don't think this is the case.
I'll ramp down to 0 at 8A/min to open and inspect. My measurements don't make any sense without both the pyrometer and the anode leakage current reading.
Tuesday, September 15, 2020, 15:49: Auto-cooling TGHT/TBHT to 0A at 8A/min (2A /15 s).
Tuesday, September 15, 2020, 16:00: Auto-cooling aborted, the system is no longer current limited. The contact causing the issue probably moved while cooling.
***many ramp ups.downs, Temperature measurements, voltage sweeps, inverse temperature estimations. Absolute temperature measurements for when the vanadium wire melted, the pyrometer was already reading 1920, a slightly adjust on the emissivity slope move it to 1911C
Tuesday, September 15, 2020, 18:47: Ramp down TGHT/TBHT to 500/250 A @ -1A/min
Tuesday, September 15, 2020, 18:48: Done for today.
Wednesday, September 16, 2020, 10:02: Auto-ramp up TGHT/TBHT to 580/285 A @ 2A/min
Wednesday, September 16, 2020, 12:59: Auto-ramp up TGHT/TBHT to 600 A @ 2 A/min
Wednesday, September 16, 2020, 13:45: Auto-ramp up TBHT to 290 A @ 1A/min
Wednesday, September 16, 2020, 18:45: Auto-ramp down TGHT/TBHT to 400/200 A @ -2A/min
Thursday, September 17, 2020, 08:46: Auto-ramp up TBHT to 285 A @ 2A/min
Thursday, September 17, 2020, 12:03: Auto-cooling TGHT/TBHT to 0A @ -4A/min
Thursday, September 17, 2020, 13:49: Turbo off. Roughing pump off |
Saturday, September 05, 2020, 21:33, Marla Cervantes, Empty, , , Done, Pristine Ta tube calibration
|
Saturday, September 05, 2020, 12:56
A Ta tube was wrapped with 3 tantalum foils,
a tantalum cap was inserted in both sides of the Ta tube, the caps weren't sealed.
The tube was set in the EVAP2
IGP1 = 3.6e-7 Torr
Saturday, September 05, 2020, 12:57
Autoram set to 10A/30 s to 200 A
Saturday, September 05, 2020, 13:11
TGHT = 2.7 V, 198.9 A
IGP1 =3e-6 Torr
Autoramp set to to 300 A at 5A/30s
Saturday, September 05, 2020, 14:45
IGP1 = 5.1e-7 torr
TGHT = 4.5 V, 303 A
Oemga = 1259 C,
AP = 1233.5 C
Autoramp set to 450A at 5 A/30s
Saturday, September 05, 2020, 15:05
TGHT = 7.3 V, 457.7 A
IGP1 = 2.8e-6 Torr
Omega = 1722 °C
AP = 1572.2 °C
Saturday, September 05, 2020, 15:16
TGHT = 9.2 V, 552.5 A
IGP1 = 7.5e-6 Torr
Omega = 2016 °C
AP= 1735.9 °C
Saturday, September 05, 2020, 21:33
IGP1 = 1.1e-6 Torr
TGHT = 11.2 V, 651.9 A
Omega = 2300 °C |
Monday, August 31, 2020, 12:57, Marla Cervantes, , 44489-15 , , Done, TaC coating heating test
|
Monday, August 31, 2020, 12:23
A short naked Ta tube (no heat shielding), previously coated with TaC was set under vacuum,
and it will be kept at 2000 °C for 3 days to later identify the TaC's carbon penetration.
Currently pumping down.
Tuesday, September 01, 2020, 12:25
IGP1 = 2.0-7 Torr
Good vacuum = 3e-2 Torr
Bad vacuum = 5e-2Torr
Autoram set to 200A at 10A/30 s
Tuesday, September 01, 2020, 12:36
IGP1 = 5.2e-7 Torr
Autoramp set to 300 A at 5 A/30 s
Tuesday, September 01, 2020, 14:11
IGP1 = 3.4e-7 Torr
TGHT = 330.2 A, 4.2 V
Omega = 1234 °C
Tuesday, September 01, 2020, 14:31
IGP1 = 1.76e-6 torr
TGHT = 6.94 V, 510 A
Oemga = 1564 C,
AP = 1390.2 C
Autoramp set to 600 A at 5 A/30s
Tuesday, September 01, 2020, 15:33
TGHT power supply = 600 A, 8.74 V
Omega = 1807 C
Autoramp set to 700 A at same rate
Tuesday, September 01, 2020, 15:33
TGHT power supply = 11.94 V, 765 A
Omega = 2157 °C
Wednesday, September 02, 2020, 10:15
IGP1 = 1.0e-6 Torr
TGHT = 12.0 V, 772 A
Omega = 2167 °C
Wednesday, September 02, 2020, 13:26
IGP1 = 9.1e-7 Torr
TGHT = 12 V, 769.5 A
Omega = 2166 °C
Wednesday, September 02, 2020, 16:06
IGP1 = 8e-7 Torr
TGHT = 12 V, 773.3 A
Omega = 2167 °C
Wednesday, September 02, 2020, 20:53
IGP1 =7.4e-7 Torr
TGHT = 11.8 V, 760.95 A
Omega = 2164 °C
Thursday, September 03, 2020, 09:54
IGP1 = 5.5e-7 Torr
TGHT = 11.9 V, 774 A
Omega = 2162 °C
Thursday, September 03, 2020, 11:06
IGP1 = 5.3e-7 Torr
TGHT = 11.9 V, 758.7A
Omega = 2161 °C
Thursday, September 03, 2020, 14:39
IGP1 = 4.8e-7 Torr
TGHT = 11.9 V, 771.8 A
Omega = 2164 °C
Friday, September 04, 2020, 09:34
IGP1 = 3.9e-7 Torr
TGHT = 11.9 V, 760.1 A
Omega = 2168 °C
Friday, September 04, 2020, 13:39
IGP1 = 3.5e-7 Torr
TGHT = 11.9 V, 758.6 A
Omega = 2170 °C
Friday, September 04, 2020, 15:55
IGP1 = 3.5e-7 Torr
TGHT = 12 v, 760.6 a
Omega = 2171 °C
|
Sunday, August 30, 2020, 18:28, Marla Cervantes, Empty, 44489-13, , Done, TaC coating/sintering
|
Sunday, August 30, 2020, 06:47
A short tantalum tube was coated with TaC and wrapped with 3 layers of Ta,
a Ta cap was inserted to the end of the tube to be able to measure the temperature during heating
Desired temperature= 1900 C,
Omega Slope set = 0.990
Sunday, August 30, 2020, 06:48
IGP1 = 3.9e-7 Torr
Autoramp set to 0.5A/min to 400 A
Sunday, August 30, 2020, 18:27
IGP1 8.41e-7 Torr
TGHT = 4.2 V, 327.15 A
Omega = 1367 °C
Sunday, August 30, 2020, 18:49
IGP1 = 9.6e-7 Torr
TGHT = 4.4 V, 337.1 a
Omega = 1402 °C
Sunday, August 30, 2020, 19:25
IGP1 = 9.5e-7 Torr
TGHT = 4.6 A, 347.5 A
Omega = 1472 °C
Autoramp set to 450 A at 0.1A/30s
Sunday, August 30, 2020, 19:59
IGP1 = 8.5e-7 Torr
TGHT = 4.8 V, 360.5 A
Omega = 1510 °C
Sunday, August 30, 2020, 22:07
IGP1 = 7.2e-7 Torr
TGHT = 5.3 V, 392.6 A
Omega = 1675 °C
Sunday, August 30, 2020, 22:16
IGP1 = 7.1e-7 Torr
TGHT = 5.5 V, 403.2 A
Omega = 1678 °C
Autoramp set to 450 at 0.1A/min
Sunday, August 30, 2020, 22:26
IGP1 = 6.9e-7 Torr
TGHT = 5.5 V, 399.15 A
Omega = 1689 °C
Monday, August 31, 2020, 08:08
IGP1 = 4.4e-7 Torr
TGHT = 6.4 V, 453.4
Omega = 1852 °C
Monday, August 31, 2020, 08:12
Autorap set to 0 A at -5 A/min |
Wednesday, August 26, 2020, 10:27, Marla Cervantes, , 44489-8, , Done, C-Cartridge test #2
|
Wednesday, August 26, 2020, 10:26
A Ta short tube was loaded with a C-cartridge
Currently, the tube is under vacuum and it will be heated to 2000 °C during 3 days.
IGP1 = 3.2e-7 Torr
Wednesday, August 26, 2020, 16:15
IGP1 = 2.5e-7 Torr
Good vacuum = 3e-2 Torr
Bad vacuum = 5e-2Torr
Autoram set to 200A at 10A/30 s
Wednesday, August 26, 2020, 17:05
TGHT = 3.9 V, 301.3 A
IGP1 = 5.4e-7 torr
Omega = 1378 °C
AP (slope 0.9) = 1441.8 °C
Wednesday, August 26, 2020, 17:20
Autoramp set to 550 A at 5A/30s
Wednesday, August 26, 2020, 23:43
TGHT = 7.561 V, 504.9 A
Omega = 2124 °C
AP = 2010.5 °C
Thursday, August 27, 2020, 07:15
TGHT = 7.461 V, 510.2 A
Omega = 2103 °C
Thursday, August 27, 2020, 13:41
TGHT = 7.5 V, 510.8 A
Omega = 2099 °C
Friday, August 28, 2020, 09:24
TGHT = 7.4 V, 513.9 A
Omega = 2103 °C
Friday, August 28, 2020, 13:12
TGHT = 7.46 V, 505.6 A
IGP1 = 2.7e-7 Torr
Omega = 2103 °C
Saturday, August 29, 2020, 14:18
IGP1 = 2.5e-7 Torr
TGHT = 7.5 V, 510.8 A
Omega = 2109 °C
Saturday, August 29, 2020, 17:44
IGP1 = 2.4e-7 Torr
TGHT = 7.5 V, 505.2 A
Omega = 2119 °C
Saturday, August 29, 2020, 17:51
Starting ramp down to 0 A at 5 A/min |
Saturday, August 22, 2020, 11:44, Marla Cervantes, , 44489-11, , Done, C-Cartridge test#1
|
Saturday, August 22, 2020, 11:41
A Ta short tube was coated with TaC and sintered, then it was loaded with a c-cartridge
Now is currently under vacuum and it will be heated to 2000 °C during 3 days
Saturday, August 22, 2020, 11:43
Good vacuum = 3e-2 Torr
Bad vacuum = 5e-2Torr
IGP1 = 3.08e-7 Torr
Autoram set to 10A/30 s to 200 A
Saturday, August 22, 2020, 11:59
Good vacuum = 3e-2 Torr
Bad vacuum = 5e-2Torr
TGHT = 2.36 V, 200.1 A
IGP1 =2.46e-6 Torr
Autoramp set to to 300 A at 5A/30s
Saturday, August 22, 2020, 13:03
TGHT = 7.32 V, 495.3 A
IGP1 = 2.7e-6 Torr
Omega = 2016 °C
AP = 1970.1 °C
Autoramp set to 550 A at 5A/30s
Saturday, August 22, 2020, 13:11
TGHT =7.6 V, 523.2 A
IGP1 = 3.2e-6 Torr
Omega = 2077 °C
Monday, August 24, 2020, 07:59
Voltage increased ~0.2 V while current remained the same indicating an increment in resistance, temperature increment increased accordingly
TGHT = 7.815 V, 520.87 A
Omega = 2126 °C
Monday, August 24, 2020, 08:04
The current was reduced 0.1 A to 519.9
Monday, August 24, 2020, 08:55 Omega = 2112 °C
Monday, August 24, 2020, 09:12
The temperature returned to Omega = 2130 °C
The current was reduced 0.1 A to 519.8
Monday, August 24, 2020, 09:56
TGHT = 7.7 V, 518.3 A
Omega = 2132 °C
Monday, August 24, 2020, 09:59
The current was reduced 0.2 A to 519.6 A
TGHT = 7.7 V, 517.3 A
Monday, August 24, 2020, 10:07 Omega = 2130°C
Monday, August 24, 2020, 10:08
The current was reduced 0.4 A to 519.2 A
TGHT = 7.7 V, 513.5 A
Monday, August 24, 2020, 10:13 Omega = 2129°C
Monday, August 24, 2020, 10:21
Voltage dropped to 7.6 V and temperature reduced to 2105 °C
Monday, August 24, 2020, 10:30
Voltage increased to 7.8 V and temperature increased to 2128 °C
Monday, August 24, 2020, 10:33
The current was reduced 0.4 A to 518.6 A
TGHT = 7.7 V, 513.06 A
Monday, August 24, 2020, 10:38 Omega = 2130 °C
Monday, August 24, 2020, 10:41
The current was reduced 0.4 A to 518.2 A
Monday, August 24, 2020, 10:52 Omega = 2134 °C
Monday, August 24, 2020, 11:13
The current was reduced 0.4 A to 517.8 A
Monday, August 24, 2020, 11:19 Omega = 2128 °C
Monday, August 24, 2020, 11:19
The current was reduced 0.4 A to 517.4 A
Monday, August 24, 2020, 11:22 Omega = 2126
Monday, August 24, 2020, 11:22
The current was reduced 0.4 A to 517.0 A
Monday, August 24, 2020, 11:25 Omega = 2123 °C
Monday, August 24, 2020, 11:26
The current was reduced 0.4 A to 516.6 A
Monday, August 24, 2020, 11:30 Omega = 2109 °C
Monday, August 24, 2020, 11:30
The current was reduced 0.4 A to 516.2 A
Monday, August 24, 2020, 11:36 Omega = 2100 °C
Monday, August 24, 2020, 11:37
The current was reduced 0.4 A to 516.0 A
TGTH = 7.5 V, 512.9 A
Omega = 2095 °C
Monday, August 24, 2020, 14:17
Voltage dropped and later on increased
TGHT = 7.7 V, 517.5 A
Omega = 2120 °C
Monday, August 24, 2020, 14:18
The current was reduced 0.4 A to 515.6 A
TGHT = 7.6 V, 509.4 A
Monday, August 24, 2020, 14:20 Omega = 2125 °C
Monday, August 24, 2020, 14:20
The current was reduced 0.4 A to 515.2 A
Monday, August 24, 2020, 14:22 Omega = 2122 °C
Monday, August 24, 2020, 14:22
The current was reduced 0.4 A to 514.8 A
Monday, August 24, 2020, 14:29 Omega = 2116 °C
Monday, August 24, 2020, 15:27
The voltage dropped as well as the temperature
TGHT = 7.5 V, 512.5 A
Monday, August 24, 2020, 15:28 Omega = 2095 °C
Monday, August 24, 2020, 22:06
TGHT = 7.6 V, 515.9 A
Omega = 2105 °C
Tuesday, August 25, 2020, 09:07
TGHT = 7.6 V, 519.13 A
Omega = 2102 °C
Tuesday, August 25, 2020, 13:02
TGHT = 7.6 V, 518.0 A
Omega = 2116 °C
IGP1 = 3e-7 Torr
Tuesday, August 25, 2020, 13:04
Starting ramp down to 0 A at 5 A/min |
Tuesday, August 18, 2020, 10:41, Marla Cervantes, TaC, 44489-11, , Done, TaC coating/sintering
|
Thursday, August 19, 2020, 17:28
A short tantalum tube was coated with TaC and wrapped with 3 layers of Ta,
a Ta foil was attached to the end of the tube to be able to measure the temperature during heating
Desired temperature= 1900 C,
Omega Slope set = 0.990,
Thursday, August 20, 2020, 17:29
IGP1 = 4.25 e-7 Torr
Autoramp set to 0.5A/min to 400 A
Thursday, August 20, 2020, 20:36
IGP1 = 6.78e-7 Torr
TGHT = 267.7 A, 3.28 V
Autoramp set to 0.4 A/min to 450 A
Friday, August 21, 2020, 10:28
IGP1=7.23e-7 torr
TGHT = 6.3 v, 446.3 A
Omega = 1603 °C
Autoramp set to -5 A/min |
Tuesday, August 18, 2020, 09:26, Marla Cervantes, TaC, 44489-15, TARGET BOAT, Done, TaC coating/sintering
|
Tuesday, August 18, 2020, 09:06
A short tantalum tube was coated with TaC and wrapped with 3 layers of Ta,
a Ta foil was attached to the end of the tube to be able to measure the temperature during heating
Desired temperature= 1900 C,
Omega Slope set = 0.990,
IGP1 = 3.75e-7 Torr
Autoramp set to TGHT at 0.2 A/min to reach 52 A
Tuesday, August 18, 2020, 13:47
IGP1= 6.8e-7 Torr
TGHT =0 .511 V, 51.3 A
IGP1 = 6.8e-7 Torr
Autoramp set to TGHT at 0.5 A/min to reach 100 A
Tuesday, August 18, 2020, 20:39
IGP1 = 3.3e-7 Torr
Autoramp set to TGHT at 0.5 A/min to reach 430 A
Wednesday, August 19, 2020, 06:57
Autoramp stopped at 402 A
IGP1 = 1.12e-6 Torr
TGHT = 5.6 V, 403.65 A
Autoramp set to TGHT at 1 A/min to reach 500 A
Wednesday, August 19, 2020, 08:59
IGp1 = 1.7e-6 Torr
TGHT = 7.22 V, 500.34 A
After 30 min at 1900 °C, autoramp set to TGHT at -1 A/min to reach 450 A, the ramp will be stopped when the temperature reads 1850 °C
Autoramp stopped at 1845 °C
IGP1 = 1.17e-6 Torr
TGHT = 6.8 V, 472.95 A |
Wednesday, August 12, 2020, 11:57, Marla Cervantes, Empty, 44489-9, TARGET BOAT, Done, Pristine Ta tube calibration
|
Short oven loaded with additional hardware are spacers into the flex-line HS.
A Ta short tube was wrapped with 3 tantalum foils,
a tantalum cap was inserted in both sides of the Ta tube, the caps weren't sealed.
The tube was set in the EVAP2
Wednesday, August 12, 2020, 11:48: Electrical check in EVAP 2:
Target to HS @ 563V
Leg to leg above bracket
TGHT A @ 10A: 1.332 mOhm
TGHT B @ 10A: 1.300 mOhm
Leg to leg w/ bracket
TGHT A @ 10A: 1.490 mOhm
TGHT B @ 10A: 1.491 mOhm
Wednesday, August 12, 2020, 12:08: Roughing.
Wednesday, August 12, 2020, 2:08: Turbo.
Thursday, August 13, 2020, 09:14
IGP1 = 7.9e-7 Torr
A leak check was performed, no leak detected.
TGHT power supply on.
Thursday, August 13, 2020, 10:03
IGP1 = 7.7e-7 Torr.
The current was tapped to 50 A
Autoramp set to 1 A each 10 s to 200 A
Good vaccum 3e-5 Torr
Bad vacuum 5e-5 torr
Thursday, August 13, 2020, 10:47
Autoramp reached 200 A
TGHT = 200.25 A, 2.38 V
IGP1 = 1.58e-6 Torr
Thursday, August 13, 2020, 11:07
TGHT = 200.25 A, 2.38 V
IGP1 = 9.66e-7 Torr
Target is shinning dimly
Omega reads 1033 +-50 degC
ARIEL pyrometer is installed in the back of the EVA2 to measured the body temperature of the oven
Thursday, August 13, 2020, 15:30
The connection of the pyrometer with the software was not possible to establish and delay the ramp up of the oven
Friday, August 14, 2020, 10:47
Restarting experiment,
IGP1 = 4.24e-7 Torr
TGHT = 0 A, ) V, (TGHT was ramped down)
Autoramp set to 1 A each 10 s to 200 A
Good vaccum 3e-5 Torr
Bad vacuum 5e-5 torr
Friday, August 14, 2020, 11:48
Target is shinning dimly
Omega reads 1033 +-50 degC
Autoramp set to 1 A each 10 s to 250 A
Autoramp set to 5 A each 60 s to 450 A
Friday, August 14, 2020, 13:51
TGHT = 6.46 V, 450.13 A
IGP1 = 2.32e-6 Torr
Omega = 1931 °C (slope 0.99)
ARIEL pyrometer = 1504.5 °C (slope 0.929)
Friday, August 14, 2020, 14:06
Autoramp = 5A each 2 min until 500
Autoranp stopped at 475 A (EPICS TGHT = 6.87V, 476.663A)
Omega = 2013 °C
ARIEL pyrometer = 1547 °C
Friday, August 14, 2020, 17:34
Autoramp is set to 5A each 2 min until 500
TGHT = 7.403 V, 500.006 A,
omega = 2104 C
AP= 1586 C
Friday, August 14, 2020, 17:49
Autoramp is set to 5A each 2 min until 550
Autoramp stopped by itself at 545 A instead of 550 A
TGHT = 8.11V, 547.65A,
omega = 2214C
AP= 1656.8 C
IGP1=6.8e-6 Torr
Friday, August 14, 2020, 18:13
Autoramp is set to 10A each 2 min until 600
Friday, August 14, 2020, 21:42
TGHT = 9.213 V, 597.8 A,
IGP1 3.27e-6 Torr
Omega = 2380 °C
Ramping down at 5 A per min to 475 A
Monday, August 17, 2020, 09:02
TGHT = 6.741 V, 471.6 A,
IGP1 = 3.46e-7 Torr
Omega = 2052 6°C
Proceeded to ramp down at 5 A per min to 0 A |
Wednesday, August 12, 2020, 08:58, Aaron Schmidt, , , , In progress, Install Flex line HS
|
Flex line HS installed. New SS gaskets.
Wednesday, August 12, 2020, 08:56: Roughing (Check).
Wednesday, August 12, 2020, 09:17: Ready for turbo pump.
Wednesday, August 12, 2020, 09:20: BP1 Off. Venting. |
Tuesday, August 11, 2020, 10:17, Ferran Boix Pamies, Empty, 41882-1, TARGET BOAT, In progress, Contamination foils temperature test
|
The target was prepared and put under vacuum on 2020-08-10
2020-08-11 10:16am The pressure is 1e-6Torr. Leak checked performed, water on no problem. Starting to set target heating curve. 1A/10s up to 300A
2020-08-11 11:23am target at 300A-1200degC Temperatures on exposed foil show to be higher than expected. 300degC already, 70degC on covered by foil thermocouple. Putting 50 more amps at 1A/10s
2020-08-11 12:11pm target at 350A-1340degC. 350degC on exposed thermocouple. Ramping to 400A 1A/10s.
2020-08-11 12:28pm target at 400A-1420degC. 400degC on exposed thermocouple. Ramping to 450A 1A/10s. |
Wednesday, August 05, 2020, 19:14, Ferran Boix Pamies, Empty, 41882-1, TARGET BOAT, Done, Parasitic target cooling test
|
2020-08-05 7.13pm Roughing pump on
2020-08-06 10:48am Turbo was turned on by Marla in the morning. Vacuum IGP1 4e-6Torr. Water leak check performed, everything good to start heating up target. Waiting for Anders confirmation to start.
2020-08-06 4:38pm after changing setup to metallic connections only. Roughing on. After some minutes abnormal behavior in vacuum.
Turning water off to see if it is a small water leak.
Water purged, no change in vacuum.
IEVAP2:RV1 was closed. After opening, normal vacuum behavior recovered. The valve is automatically closing when reaching 100Torr. Wasn't doing that before. Turbo on now.
2020-08-07 9:24am pumping over night, vacuum at 8e-7torr. Everything ready for test. Ramping up target heater.Up to 50A 1A/20s
2020-08-07 9:48am all good at 50A, ramping to 250 1A/10s
2020-08-07 10:27am all good at 250A, ramping to 400 1A/10s
2020-08-07 10:57am all good at 400A, ramping to 500 1A/10s
2020-08-07 11:17am Tc type C might have been deatached at 500A, ramping to 600 1A/10s
2020-08-07 11:37am All good, ramping to 700 1A/10s
2020-08-07 11:58am 1950degC on pyrometer, 1200degC on type C TC (probably not well attached anymore), TCs on heatshield [30-40]degC. Pressure 9e-6Torr
2020-08-07 12:44pm All values stable after 45min, starting to ramp up parasitic target heating elements.
2020-08-07 1:15pm Open circuit, would seem that one of the heating elements cracked. Cooling down the target.
|
Wednesday, August 05, 2020, 13:38, Aaron Schmidt, , , , , RP Swap on EVAP 2
|
BP1 swapped with RP2 (TS beamline)
U-line installed.
Wednesday, August 05, 2020, 13:37: Roughing.
Wednesday, August 05, 2020, 13:39: Open RV1 to EVAP 2 chamber.
Wednesday, August 05, 2020, 14:08: Turbo pump on.
Wednesday, August 05, 2020, 14:17: Turbo pump on (green) / Shut - off.
Wednesday, August 05, 2020, 14:18: BP1 off. Runs ok. |
Friday, July 31, 2020, 11:16, Ferran Boix Pamies, Empty, 41882-1, TARGET BOAT, Done, Thermocouple measurent of boat temperature
|
Boat with attached thermocouple type C with AREMCO ceramabond glue installed in evap2 the 30-07-2020
Vacuum 3.2e-6torr in IGP1 after night with the roughing pump and morning with turbo.
TGHT heater on.
ramp up started
1A/20s up to 200A
Thermocouple de-attached at about 400A.
Target cooled down. 1A/10s
Turbo and roughing pump off. System left with present vacuum over night. Tomorrow inspection. |
Saturday, July 25, 2020, 08:58, Darwin Ortiz Rosales, ZrC, 44139-7-SK, , In progress, ZrC for Luca's experiments
|
Friday, July 24, 2020, 15:00
Ta tube cotaining 497 ZrC discs wrapped with Ta heat-shields (3 layers)
Desired temperature= 1800C (expected TGHT 410 A), TBHT will be set fixed at 230A (max).
good vacuum = 3.00 e-05 Torr
bad vacuum = 5.00 e-05 Torr
Evap 2 was left to pump down over night.
Saturday, July 25, 2020, 08:57
IGP1= 8.7 e-07 Torr
Start ramp at 0.25 A/min to 20 A on TGHT
Saturday, July 25, 2020, 10:07
IGP1= 2.7e -06 Torr
Set ramp target to 30 A
Wednesday, July 29, 2020, 13:11
OMEGA reading 1700 C at 430 A during the night. It was kept at this temperature for 3.5 hours. The OMEGA slope was not changed from 0.990
when IGP1 = 1.2 e-06 Torr and stable, cooling was started at -3A/min at 9 am on this day.
IGP1= 2.2 e-07 Torr now at time of dismounting
|
Monday, July 20, 2020, 19:25, Darwin Ortiz Rosales, SiC, 44139-11, LP-SIS, Done, SiC sintering for Luca 2 of 2
|
Monday, July 20, 2020, 19:27
Coated Ta tube cotaining 355 SiC disks wrapped with Ta heat-shields (3 layers)
Desired temperature= 1800C (expected TGHT 410 A), TBHT will be set fixed at 230A (max).
good vacuum = 3.00 e-05 Torr
bad vacuum = 5.00 e-05 Torr
Evap 2 was left to pump down over night.
Monday, July 20, 2020, 23:06
IPG1 = 3.1e-06 Torr
Start autoramp at .25A/min to 40A for both TGHT and TBHT
Tuesday, July 21, 2020, 08:06
TGHT = 40.3 A, 0.51 V
TBHT = 39.0 A, 0.46 V
increase auto ramp limit to 50 A for both TGHT and TBHT
IGP1=1.8e-05 Torr
Tuesday, July 21, 2020, 16:22
IGP1= 1.5 e-05 Torr
TGHT = 50.1 A, 0.65 V
TBHT = 50.0 A, 0.60 V
Change ramp target to 350 A for TGHT and 230A for TBHT
Wednesday, July 22, 2020, 13:24
Stopped autoramp. Will allow pressure to drop.
TGHT = 64.0 A, 0.86 V
TBHT = 64.5 A, 0.82 V
Thursday, July 23, 2020, 23:55
TGHT Reached 430 A, 7.7 V
OMEGA reads 1310 C but reading is not considered accurate so will leave at this current for 4 hours.
Friday, July 24, 2020, 11:31
IGP1 = 1.98e-07 Torr
Window for pyrometer was coated with condensate.
Dismounted target and cleaned two windows in line with the pyrometer.
|
Thursday, July 16, 2020, 11:15, Darwin Ortiz Rosales, SiC, 44139-11, LP-SIS, Done, SiC sintering for Luca 1 of 2
|
Thursday, July 16, 2020, 11:15
Coated Ta tube cotaining 233 SiC disks wrapped with Ta heat-shields (3 layers)
Desired temperature= 1800C (expected TGHT 410 A), TBHT will be set fixed at 230A (max).
Evap 2 was pumped down
Friday, July 17, 2020, 08:49
Total length packed approximately 10 cm
container has 3 Ta heat shields.
No endcaps inserted to facilitate out-gassing
Two TaC coated Ta wire springs inserted at both ends.
Initially to ramp TGHT and TBHT to 40 A at 0.5 A/min
Then heat ramping TGHT manually and automatically to reach 400 A (Omega slope set = 0.990)
Then ramp to temperature = 1800 C
TBHT will be set fixed at 230 A (max). TBHT heated manually and automatically to max.
Good vac at 3.00 e -5 Torr
Bad vac at 5.00 e-5 Torr
Initial IGP1 = 6.45e-07 Torr
Friday, July 17, 2020, 20:49
TBHT = 38.9 A, 0.47 V
TGHT = 39.7 A, 0.59 V
IGP1 = 9.1e-06 Torr
Autoramp to 50 A at 0.5 A/min for both TGHT and TBHT
Saturday, July 18, 2020, 09:04
IGP1 = 1.6e-06 Torr
TGHT = 50.5 A, 0.76V
TBHT = 49.7 A, 0.62 V
Starting autoramp at 0.5 A/ min to 400 A TGHT and 230 A TBHT
Saturday, July 18, 2020, 10:17
IGP1 = 5.06e-05 torr
stopped autoramp and allow pressure to decrease and stabilize
Saturday, July 18, 2020, 10:47
IGP1 = 6.65 e-06 Torr and trending down
TGHT = 55.4 A, 0.83 V
TBHT= 54.6 A, 0.68 V
Change autoramp to 0.25 A/min for both heaters (.05 increments and 120s wait)
Sunday, July 19, 2020, 08:46
IGP1= 2.2 e-05 Torr
TBHT = 109.5 A, 1.6 V
TGHT = 106.6 A, 1.7 V
increased ramping rate to .5A/min by decreasing wait intervals to 60 s
Sunday, July 19, 2020, 14:55
IGP1 = 7.1 e -06 Torr
TGHT = 271.8 A, 4.7 V
TBHT = 233.1 A, 4.1 V
Increasing ramping rate to 1 A/min
Sunday, July 19, 2020, 17:35
IGP1 = 2.6e-06 Torr
TGHT = 400 A, 7.2 V
TBHT = 233 A, 4.1 V
Tap manually to 410 (expected 1800 C )
Note* OMEGA reading cannot be obtained.
Leave at 410 A on TGHT for 4 hours.
Sunday, July 19, 2020, 22:57
IGP1 = 7.0 e-07 Torr
TGHT= 410 A , 7.2 V
TBHT = 233 A, 4.2 V
Start cool down at -2A/min for TGHT and -1A/min for TBHT
Monday, July 20, 2020, 12:20
IGP1 = 2.2e-07 Torr
Unloading target |
Monday, July 13, 2020, 11:03, Aaron Schmidt, , , , , Pump down / leak / vacuum check.
|
Darwin reported that he was unable to achieve vacuum of 150mTorr. The flex-line HS had been removed last week for modifications. SS gaskets received today. Replaced HS gaskets (Cu).
Monday, July 13, 2020, 11:00: Roughing.
Monday, July 13, 2020, 11:44: Vacuum to 200mTorr. Venting.
Monday, July 13, 2020, 11:55: Roughing. HS waterlines were opened. No visible leak detected.
Monday, July 13, 2020, 12:32: Venting. Vacuum to 175mTorr.
Monday, July 13, 2020, 12:34: Roughing.
Monday, July 13, 2020, 15:21: Turn off the roughing pump. Vent in the am & plan to remove the HS to leak check the HS & EVAP 2.
Tuesday, July 14, 2020, 07:42: Venting.
Tuesday, July 14, 2020, 08:23: Flexible line HS removed. U-Line installed. Roughing.
Tuesday, July 14, 2020, 08:54: Turbo pump on.
Tuesday, July 14, 2020, 11:15: Vacuum @ 3.14e-06T. Turbo & Roughing pump off.
Tuesday, July 14, 2020, 11:25:
HS leak checks:
0.0e-08 atm-cc/sec
0.0e-07 atm-cc/sec @ 75 PSI He w/ sniffer.
0.0e-07 atm-cc/sec @ 120 PSI He w/ sniffer. (Note HS is very dirty inside)
Tuesday, July 14, 2020, 11:35: Venting EVAP 2. He bottle connected on "Air-In" on the HS water supply line.
Tuesday, July 14, 2020, 13:50:
Pressurized the HS lines on EVAP 2 w/ 30 PSI He for 10 minutes. Remained @ 0.0e-07 atm-cc/sec.
Tuesday, July 14, 2020, 13:53: Roughing.
Tuesday, July 14, 2020, 17:33: Turbo pump on.
Wednesday, July 15, 2020, 10:31: Turbo pump off.
Wednesday, July 15, 2020, 12:02: HS Leak checked in the cold lab: 0.0e-07 atm-cc/sec @ 120 PSI He w/ sniffer.
Wednesday, July 15, 2020, 12:34: Venting.
Wednesday, July 15, 2020, 13:37: Installed flex-line HS. Pressurized the HS lines on EVAP 2 w/ 30 PSI He for 10 minutes. Remained @ 0.0e-07 atm-cc/sec.
Wednesday, July 15, 2020, 13:42: Roughing.
Wednesday, July 15, 2020, 14:16: Turbo pump on.
Wednesday, July 15, 2020, 15:59: Vacuum @ 3.85e-06T
Wednesday, July 15, 2020, 16:00: Waterline opened. No immediate response on Vacuum.
Wednesday, July 15, 2020, 16:03: Vacuum @ 3.69e-06T and continuing to drop. |
Monday, June 15, 2020, 14:28, Darwin Ortiz Rosales, Empty, 42218-7, HP-SIS, Done, TaC coating/sintering
|
Monday, June 15, 2020, 13:30
Container coated with TaC and wrapped with 3 Ta heat shields.
Desired temperature= 1900 C, Omega Slope set = 0.990, Auto TGHT at 0.2A/min to reach 400A, TGHT will be tapped up accordingly to reach desired Temp.
TBHT will be set fixed at 230 A max).
Good vac at 3.00e -5 Torr
Bad vac at 5.00e-5 Torr
Chamber pump down
Tuesday, June 16, 2020, 08:55
IGP1= 4.2e-7 Torr
Starting ramp to 50A at 0.2A/min for both TGHT and TBHT. Observing pressure behaviour.
Tuesday, June 16, 2020, 14:14
IGP1 = 9.0e-7 Torr
TGHT = 50.3 A, 0.6 V
TBHT = 49.4 A, 0.54 V
Set TGHT to 400A and TBHT to 230A
Tuesday, June 16, 2020, 16:58
IGP1 = 7.32e-7 Torr
TGHT = 82.3A, 1.0 V
TBHT = 81.8 A, 0.96V
Will try to increase ramp rate to 2 A/min for both TGHT and TBHT
Tuesday, June 16, 2020, 17:30
Pressure spike.
IGP1 = 2.5e-5Torr
TGHT = 44.1 A, 0.57 V
TBHT = 43.0 A, 0.49 V
Will return to 0.2A/ min ramp rate for both heaters
Thursday, June 18, 2020, 20:26
Autoramped to 720A , 11.6V on TGHT at 0.2A/min
OMEGA = 1850C
Manually ramped to 740 A , on TGHT while TBHT remains at 230A
OMEGA= 1885 C
IGP1=4.6e-06 Torr trending down
Will remain at this temperature for next 4 hours
NOTE* Current on TGHT very unstable (oscillates)
Friday, June 19, 2020, 11:31
Last night at 00:15 am started cooling TGHT at -2A/min and TBHT at -0.2 A/min
(The elog entry was not submitted and computer restarted overnight so notes were lost).
at 6:30 am Friday June 19, 2020
Increased TBHT cooling to -2A/min and decreased THGT cooling to -1A/min
Monday, June 22, 2020, 13:54
IGP1= 8.1e-8 Torr
Evaporator vented and container pulled out. There is slight peeling near one end of the container. This area should be on the outside of the end-caps so the container should be usable.
Files to be uploaded later.
|
Thursday, June 11, 2020, 13:01, Darwin Ortiz Rosales, Empty, 44139-12, LP-SIS, Done,
|
Thursday, June 11, 2020, 09:56
Previous day (Wednesday June 10, 2020)
Container coated with TaC and wrapped with 3 Ta heat shields.
Desired temperature= 1900 C, Omega Slope set = 0.990, Auto TGHT at 0.2A/min to reach 400A, TGHT will be tapped up accordingly to reach desired Temp.
TBHT will be set fixed at 230 A (max).
Good vac at 3.00e -5 Torr
Bad vac at 5.00e-5 Torr
Chamber pump down
Thursday, June 11, 2020, 10:19
IEVAP2:IGP1=1.06e-6 Torr
ramping to 40A (TGHT and TBHT) at 1A/min
Thursday, June 11, 2020, 12:35
IEVAP2:IGP1=1.8e-6 Torr
TGHT = 39.8 A, 0.45V
TBHT=38.5 A, 0.48V
Manually rampted to 45A on both TGHT and TBHT
Thursday, June 11, 2020, 12:58
IEVAP2:IGP1=1.6e-6 Torr
TGHT = 34.8 A, 0.52V
TBHT=44.2A, 0.55V
Start Autoramp at .5A/min to 400A on TGHT and 230A on TBHT
Thursday, June 11, 2020, 17:14
Irregular pressure profile. Cooling . Need to check for leak.
TGHT = 99 A 1.3 V
TBHT = 99 A 1.4 V
Friday, June 12, 2020, 12:59
Restarting ramping
IGP1= 4.98e7 Torr
Autoramp at 1A/min to 400A on TGHT and 230A on TBHT
(pressure and TGHT current and voltage profile seem normal compared to previous coating sintering with the same power supply)
Friday, June 12, 2020, 14:40
Paused ramping
TGHT = 90A
After a few minutes the profile (noise) was still there. Continue autoramp at 0.5A/min to 400 A on TGHT and 230A on TBHT
Friday, June 12, 2020, 15:21
IGP1= 1.97e-06 Torr trending down
TGHT = 111.5 A , 1.5 V
TBHT = 112.9 A, 1.9 V
Increase ramping speed to 1A/min to 400A on TGHT and 230A on TBHT
Friday, June 12, 2020, 20:50
OMEGA = 1754 C
IGP1= 2.5e-6 Torr
TGHT = 394.1 A, 6.6 V
TBHT = 232.8 A, 4.0 V
Tapping to 1900 C
Friday, June 12, 2020, 21:00
OMEGA =1901 C
IGP1= 5.6e-6 Torr
TGHT = 448.3 A, 7.5 V
TBHT = 232.8 A, 4.1 V
Saturday, June 13, 2020, 00:51
OMEGA = 1898 C
IGP1 = 2.0e-6 Torr
TGHT = 447.2 A, 7.5 V
TBHT = 232.9 A, 4.1 V
Start cooling at -2A/ min for TGHT and -1A/min for TBHT
|
Monday, June 01, 2020, 12:03, Aaron Schmidt, Ta, 44139-13, LP-SIS, In progress, Ta#60 Conditioning
|
Ta#60 LP-SIS target description:
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.025mm
Target density = 14.081 g/cm3
Target length = 3.33 cm
Total Mass = 46.891 g [Incl foils + Ta wire on 6 packs]
Total mass w/ Target oven= 445g w/ end caps)
Discs in target are arranged as follows: 1pack / 75singles / 1pack / 100singles / 2packs / 100singles / 1pack / 75singles / 1pack
End caps installed (Expanded). No Ta heat shield added.
https://elog.triumf.ca/TIS/Target+Production/98
Monday, June 01, 2020, 11:38: Roughing.
Monday, June 01, 2020, 12:03: Turbo pump on.
TBHT will be ramped up to 230A at 1.0A/min.
TGHT will be ramped up to 600A + at 2.0A/min.
Final desired temperature = 1900C.
OMEGA slope = 0.98.
Tuesday, June 02, 2020, 07:13: Omega slope set to 0.98. Power supplies / sources on. vacuum@ 5.13e-07T.
Tuesday, June 02, 2020, 07:16: Manually tap up TGHT / TBHT to 40 / 5 A. Vacuum @ 5.08e-07T.
Tuesday, June 02, 2020, 07:19: Auto-ramping TGHT / TBHT @ 2 A per min to 350 / 150 A.
Tuesday, June 02, 2020, 10:02: Auto-ramping TGHT / TBHT @ 2 / 1 A per min to 450 / 200 A. Vacuum @ 1.39e-06T. TGHT Voltage= 5.955V. Omega: 1288 deg C.
Tuesday, June 02, 2020, 11:54: Auto-ramping TGHT / TBHT @ 2 / 1 A per min to 500 / 230 A. Vacuum @ 1.85e-06T. TGHT Voltage= 7.998V. Omega: 1528 deg C.
Tuesday, June 02, 2020, 13:16: Auto-ramping TGHT @ 2 A per min to 550 A. Vacuum @ 2.51e-06T. TGHT Voltage= 9.060V. Omega: 1625 deg C.
Tuesday, June 02, 2020, 13:58: Auto-ramping TGHT @ 2 A per min to 600 A. Vacuum @ 3.53e-06T. TGHT Voltage= 9.060V. Omega: 1728 deg C.
Tuesday, June 02, 2020, 14:23: Auto-ramping TGHT @ 2 A per min to 625 A. Vacuum @ 5.56e-06T. TGHT Voltage= 11.236V. Omega: 1821 deg C.
Tuesday, June 02, 2020, 14:36: TGHT / TBHT 625 / 230 A. Vacuum @ 6.65e-06T. TGHT Voltage= 11.724V. Omega: 1865 deg C.
Tap up TGHT manually.
Tuesday, June 02, 2020, 14:48: TGHT / TBHT 643 / 230 A. Vacuum @ 7.24e-06T. TGHT Voltage= 12.129V. Omega: 1901-1903 deg C.
Desired temperature = 1900C reached.
Tuesday, June 02, 2020, 22:20: TGHT / TBHT 643 / 230 A. Vacuum @ 2.05e-06T. TGHT Voltage= 12.212V. Omega: 1901-1903 deg C.
Tuesday, June 02, 2020, 22:22: Auto-Cooling @ 1 A per min.
Wednesday, June 03, 2020, 06:08: TBHT @ 0. TGHT set for Auto-Cooling @ 2 A per min.
Wednesday, June 03, 2020, 11:38: PS off. Turbo pump off.
Wednesday, June 03, 2020, 12:40: Venting. |
Friday, May 29, 2020, 10:26, Marla Cervantes, Empty, 43044-8, LP-SIS, Done, TaC coating/sintering
|
Friday, May 29, 2020, 08:52
Ta tube was coated with TaC and wrapped with Ta heat-shields (3 layers)
Desired temperature= 1900 C (expected TGHT ~430 A), TBHT will be set fixed at 230A (max).
Evap 2 was pumped down
Good vacuum= 3.00 e-5 Torr
Bad vacuum = 5.00 e-5 Torr
Ramped TGHT and TBHT to 40A at 0.5A/min
Initial IGP1 = 3.7e-7 Torr
Friday, May 29, 2020, 10:23
Autoramp deliver 40 A
TGHT = 0.47 V, 40.72 A
TBHT = 0.5 V, 38.78 A
IGP1 = 4.5 e-6 Torr and going down
Autoramp TGHT and TBHT at 1A/min to 400A and 230A respectively.
Friday, May 29, 2020, 11:27
Autoramp was stopped at 70 A, since pressure kept increasing, current was manually decreased to 65 A in both TGHT and TBHT.
The system will remain at current conditions until pressure reduce.
Friday, May 29, 2020, 12:44
Autoramp TGHT and TBHT at 1A/min to 400A and 230A respectively.
Saturday, May 30, 2020, 00:23
Autoramp deliver 400 A at TGHT and 230 A at TBHT
TGHT = 7.8 V, 453.9 A
TBHT = 4.21 V, 232.9 A
IGP1 = 9.7 e-6 Torr and going down
Omega = 1893 degC
Autoramp TGHT and TBHT at -1A/min to 400 A
Initiating auto-cool at -2.0A/min and -1.0A/min for the TGHT and TBHT respectively
|
Wednesday, May 27, 2020, 13:04, Marla Cervantes, , 44139-7-SK, , Done, Conditioning graphite target #2
|
Wednesday, May 27, 2020, 10:22
IGP1 = 3.2e-7 Torr
TGHT = 0.186 V, 0.028 A
The autoramp is set to 50A:
1 A each 10 s with a good vacuum of 3e-2 Torr and a bad vacuum 5e-2 Torr
Wednesday, May 27, 2020, 10:40
TGHT = 1.17 V, 50.9 A
PS = 1.21 V, 50 A
IGP1 = 8e-4 Torr and going down
Autoramp is set to 80 A same conditions
1 A each 10 s with a good vacuum of 3e-2 Torr and a bad vacuum 5e-2 Torr
Wednesday, May 27, 2020, 12:29
TGHT = 1.59 V, 80.04 A
PS = 1.58 V, 80 A
IGP1 = 2e-4 Torr and going down
Autoramp is set to 100 A,conditions:
1 A each 20 s with a good vacuum of 3e-2 Torr and a bad vacuum 5e-2 Torr
Wednesday, May 27, 2020, 12:38
TGHT = 1.97 V, 100.35 A
IGP1 = 4e-4 Torr
Autoramp is set to 120 A,conditions:
1 A each 20 s with a good vacuum of 3e-2 Torr and a bad vacuum 5e-2 Torr
Wednesday, May 27, 2020, 12:48
TGHT = 2.27 V, 119.1 A
IGP1 = 4e-4 Torr
Autoramp is set to 190 A,conditions:
1 A each 10 s with a good vacuum of 3e-2 Torr and a bad vacuum 5e-2 Torr
Wednesday, May 27, 2020, 13:03
TGHT = 3.4 V, 191.25 A
IGP1 = 3e-4 Torr
Autoramp is set to 190 A,conditions:
2 A each 10 s with a good vacuum of 3e-2 Torr and a bad vacuum 5e-2 Torr
Wednesday, May 27, 2020, 13:36
TGHT = 7.8 V, 423 A
IGP1 = 3e-4 Torr
Autoramp is set to 450 A,conditions:
2 A each 10 s with a good vacuum of 3e-2 Torr and a bad vacuum 5e-2 Torr
Wednesday, May 27, 2020, 13:43
TGHT = 8.5 V, 451.6 A
IGP1 = 2e-4 Torr
Autoramp is set to 520 A,conditions:
2 A each 10 s with a good vacuum of 3e-2 Torr and a bad vacuum 5e-2 Torr
Wednesday, May 27, 2020, 14:02
TGHT = 10.3 V, 508.16 A
Power supply = 10.39 V, 506 A
Omega = 2000 degC
AP = 2046.4 degC
After 3 hours at 2000 degC, the autoramp was set to 0 A,
conditions: -2 A each 10 s.
Note: There was a voltage drop of 0.6 V (fig. elog-484-fig2) |
Sunday, May 24, 2020, 13:39, Marla Cervantes, Empty, 44139-11, LP-SIS, Done, TaC coating/sintering
|
Sunday, May 24, 2020, 06:54
Ta tube was coated with TaC and wrapped with Ta heat-shields (3 layers)
Desired temperature= 1900 C (expected TGHT ~430 A), TBHT will be set fixed at 230A (max).
Evap 2 was pumped down
Good vacuum= 3.00 e-5 Torr
Bad vacuum = 5.00 e-5 Torr
Ramped TGHT and TBHT to 40A at 0.5A/min
Initial IGP1 = 2.5e-7 Torr
Sunday, May 24, 2020, 08:24
Autoramp deliver 40 A
TGHT = 0.58 V, 39.6 A
TBHT = 0.46 V, 39.81 A
IGP1 = 2.9 e-7 Torr and increasing
Heater conditions will be hold for 15 min to account for pressure changes.
Sunday, May 24, 2020, 08:39
IGP1 = 2.7e-7 Torr and decreasing
Autoramp TGHT and TBHT at 1A/min to 400A and 230A respectively.
Sunday, May 24, 2020, 14:57
After 15 min the autoramp stopped
TGHT = 6.8 V, 394.65 A
TBHT =4 V, 232.9 A
IGP1 = 2.2e-6 Torr and going down
Omega = 1747 degC
Autoramp set to TGHT 1A/min to 450A
Sunday, May 24, 2020, 16:07
After 15 min the autoramp stopped
TGHT = 7.7 V, 448 A
IGP1 = 2.88e-6 Torr
Omega = 1886 degC
The current will be increased manually to reach 1900 deg C
Final TGHT = 7.9 V, 453.15 A (455 A input)
Omega = 1899 degC
The TGHT and TBHT will leave at current conditions until pressure reduce (approx 4 hours)
Sunday, May 24, 2020, 20:01
TGHT = 7.9 V, 456 A
TBHT = 4 V, 232.9 A
IGP1 = 1.8e-6 Torr
Omega = 1893 degC
Initiating auto-cool at -2.0A/min and -1.0A/min for the TGHT and TBHT respectively. |
Monday, March 23, 2020, 07:50, Marla Cervantes, , 41882-1, TARGET BOAT, Done, Conditioning graphite target #1 (T2)
|
Friday, March 20, 2020, 19:39
The target material is loaded in a graphite cartridge.
The graphite cartridge is placed in a new tantalum boat previously without TaC,
the Ta boat was wrapped with three new Ta heat shields.
The system is currently pumping down.
Monday, March 23, 2020, 07:49
IGP1 = 2.2e-7 Torr
Good vacuum= 3.00 e-5 Torr
Bad vacuum = 5.00 e-5 Torr
Ramping TGHT to 40A at 0.5A/min
Monday, March 23, 2020, 10:35
Due to the COVID-19, non-essential activities are wrapped up,
the conditioning of the carbon target will be postponed until further notice |
Wednesday, May 20, 2020, 12:54, Marla Cervantes, , 41882-1, TARGET BOAT, Done, Conditioning graphite target #1 (T2)
|
Marla Cervantes wrote: |
Friday, March 20, 2020, 19:39
The target material is loaded in a graphite cartridge.
The graphite cartridge is placed in a new tantalum boat previously without TaC,
the Ta boat was wrapped with three new Ta heat shields.
The system is currently pumping down.
Monday, March 23, 2020, 07:49
IGP1 = 2.2e-7 Torr
Good vacuum= 3.00 e-5 Torr
Bad vacuum = 5.00 e-5 Torr
Ramping TGHT to 40A at 0.5A/min
Monday, March 23, 2020, 10:35
Due to the COVID-19, non-essential activities are wrapped up,
the conditioning of the carbon target will be postponed until further notice
|
Wednesday, May 20, 2020, 12:50
On May 19 the pumps of EVAP2 were turned on to purge the system
Today Aaron made a leak check, for details, visit elog-481
Currently IGP1 = 8.17e-7 Torr
Thursday, May 21, 2020, 09:41
IGP1 = 4.5e-7 Torr
TGHT = 0.03 V, 0.028 A
Current will be increased manually to 10 A, and then it will be autoramp to 500 A
Whit this power supply the current increments are register since the beging
TGHT = 0.145 V, 10.35 A
During the input of the 10 A there was no anomaly with the pressure and the autoramp was set to 50A:
1 A each 10 s with a good vacuum of 3e-2 Torr and a bad vacuum 5e-2 Torr
Thursday, May 21, 2020, 10:39
The autoramp reached the 50 A set
TGHT = 0.65 V, 49.05 A
Power supply = 0.64 V, 50 A
IGP1 = 4.7e-7 Torr
Everything looks good, autoramp is set to 80 A same conditions
1 A each 10 s with a good vacuum of 3e-2 Torr and a bad vacuum 5e-2 Torr
Thursday, May 21, 2020, 10:49
The autoramp reached the 80 A set
TGHT = 1.075 V, 79.36 A
Power supply = 1.07 V, 80 A
IGP1 = 1.7e-6 Torr and increasing
Autoramp is set to 100 A,conditions:
1 A each 20 s with a good vacuum of 3e-2 Torr and a bad vacuum 5e-2 Torr
There was a jump in the vacuum e-log-482-fig-1.
Thursday, May 21, 2020, 11:01
The autoramp reached the 100 A set
TGHT = 1.4V, 99.9 A
Power supply = 1.4V, 100 A
IGP1 = 0.001 Torr and increasing
Autoramp is set to 120 A,conditions:
1 A each 20 s with a good vacuum of 3e-2 Torr and a bad vacuum 5e-2 Torr
Thursday, May 21, 2020, 11:12
TGHT = 1.75 V, 120.6 A
Power supply = 1.74 V, 120 A
IGP1 = 0.0018 Torr
The current will be hold and to let the vacuum reduce
Thursday, May 21, 2020, 11:34
TGHT = 1.8 V, 120.825 A
Power supply = 1.74 V, 120 A
IGP1 = 9.8e-5 Torr
Thursday, May 21, 2020, 11:37
Autoramp is set to 300 A,conditions:
2 A each 10 s with a good vacuum of 3e-2 Torr and a bad vacuum 5e-2 Torr
Thursday, May 21, 2020, 12:21
TGHT = 5.015 V, 298.125 A
Power supply = 5 V, 300 A
IGP1 = 4.77e-5 Torr
Omega = 1130 degC
Note: Measurments will be taken with ARIEL's pyrometer (I will call it AP in this elog).
The emmisivity this pyrometer accounts for is 0.91 for the range of 1000 C to 1800 C
Above 01800 it will use 0.93 as the emissivity
AP = 977.7 degC
|
Wednesday, May 20, 2020, 07:18, Aaron Schmidt, , , , , Check Evap 2
|
Gradually open waterlines under vacuum after period of no use.
Wednesday, May 20, 2020, 07:17: Vacuum @ 1.13e-06T
Wednesday, May 20, 2020, 07:19: Hot lab cooling water return opened. Vacuum @ 1.13e-06T.
Wednesday, May 20, 2020, 07:22: Hot lab cooling water supply opened. Vacuum @ 1.11e-06T.
Wednesday, May 20, 2020, 07:29: Vacuum remains stable @ 1.11e-06T.
|
Wednesday, March 18, 2020, 07:21, Marla Cervantes, TaC, 44139-11, LP-SIS, Done, TaC coating/sintering
|
Wednesday, March 18, 2020, 07:10
Ta tube was coated with TaC and wrapped with Ta heat-shields (3 layers)
Desired temperature= 1900 C (expected TGHT ~430 A), TBHT will be set fixed at 230A (max).
Evap 2 was pumped down on the previous night.
Good vacuum= 3.00 e-5 Torr
Bad vacuum = 5.00 e-5 Torr
Ramped TGHT and TBHT to 40A at 0.5A/min
Initial pressure IGP1 = 4.8e-7Torr
Wednesday, March 18, 2020, 09:29
After an hour pressure reduced to 5.45e-6 Torr
TGHT; 0.518 V, 40.5 A
TBHT: 0.41 V, 38.6 A
Autoramp TGHT and TBHT at 1A/min to 400A and 230A respectively.
Wednesday, March 18, 2020, 18:29
TGHT = 400A, 6.6V, TBHT= 232.9, 3.9V
OMEGA = 1240 C, this is 500 degC lower than previous LP-SIS at same conditions
https://elog.triumf.ca/TIS/Evaporator_2/464
Start autoramp to 460A on TGHT at 1A/min
Wednesday, March 18, 2020, 20:51
TGHT: 464 A, 7.75 V
Temperature 1328, I won't increase the temperature because there is a chance that the reading is 500 degC off and the target is sitting at 1828 degC instead of 1328 degC
Wednesday, March 18, 2020, 23:17
After ~4 hours at 1317 degC according to the pyrometer:
TGHT = 7.7 V, 457.8 A,
TBHT = 3.9 V, 232.9 A,
IGP1 = 1.16e-6
Commence cooling at -2A/min for TGHT and -1A/min for TBHT
Thursday, March 19, 2020, 15:53
Venting and dismounting.
The coating does not have the quality to be used online, another LP-SIS will be coated and sinter |
Monday, March 16, 2020, 13:47, Marla Cervantes, , 40282-5, TARGET BOAT, Done, Conditioning graphite target #1
|
Monday, March 16, 2020, 13:47
Target material characteristics: Graphite cast of 0.965g/cm3, 287 D-shaped discs, disc area 0.969cm2, total mass of 9.972g, length 10.657cm.
The target material is loaded in a graphite cartridge.
The graphite cartridge is placed in a tantalum boat previously coated with TaC,
the Ta boat was wrapped with two used Ta heat shields.
The system is currently pumping down.
Tuesday, March 17, 2020, 08:11
IGP1 = 3.18e-7 Torr
Current will be increased manually to 10 A, and then it will be autoramp to 500 A
During the input of the 10 A there was no anomaly with the pressure and the autoramp was set to:
1 A each 10 s with a good vacuum of 3e-2 Torr and a bad vacuum 5e-2 Torr
Tuesday, March 17, 2020, 09:03
After 30 min:
TGHT: 98.1 A, 1.48 V (the voltage is increasing)
IGP1 = 3e-4 Torr
The autoramp is set to 2 A each 10 s to 500 A
Tuesday, March 17, 2020, 09:52
At 500 A the temperature was ~1243 C
So, the autoramp was re started 2 A each 10 s to 520 A
Tuesday, March 17, 2020, 09:56
TGHT= 510 A, 9.18 V
IGP1= 8.2e-5 Torr
Pressure decreasing.
Temperature register in iR2C: 1272 C
The target will stay at 520 A for 15 min to account for thermal equilibrium, and then the current will be increased to go to 1800 C
Tuesday, March 17, 2020, 10:11
The temperature stayed at 1270 C,
The autoramp is re started: 2 A each 10 s to 600 A
Tuesday, March 17, 2020, 10:24
TGHT: 10.693 V, 588.5 A
IGP1 max 7.4e-5 Torr
Temperature after 3 min at 588.5 A: 1368 C
Tuesday, March 17, 2020, 10:34
The autoramp is re started: 2 A each 10 s to 650 A
Tuesday, March 17, 2020, 10:46
TGHT=11.99 V, 637.6 A
IGP1=5.5e-5 Torr (8e-5 Torr max)
Temperature 1459 C
The current and voltage drop 10 A and 0.3 V respectively when the autoramp is stopped
Tuesday, March 17, 2020, 10:53
The autoramp is re started: 2 A each 10 s to 700A
Tuesday, March 17, 2020, 11:04
TGHT: 13 V, 686.59 A
IGP1: 6.2e-5 Torr (Max 8.7e-5Torr)
Temperature: 1507 C
Tuesday, March 17, 2020, 11:05
The autoramp is re started: 2 A each 10 s to 800A
Tuesday, March 17, 2020, 11:16
TGHT=14.29 V, 759 A
IGP1: 8.6e-5 Torr (Max 1e-4 Torr)
Temperature 1527 C
There is a current discrepancy in EPICs (see current discrepancy picture),
the autoramp stopped at 761 A because EPICS? reads 800 A
Increasing current manually.
Increasing the current manually did not work, because set current is at fake maximum
Tuesday, March 17, 2020, 13:43
The temperature stabilized to 1567 C. The current however was not stable ( look at the CarbonTarget - Max current)
an autoramp is set to -2 A each 10 s to 0A
The set current is going down but not the epics reading current neither the temperature. I assume the current will star going down when the set and the reading current from epics are the same.
Tuesday, March 17, 2020, 13:50
Autoramp was stopped, and current was reduced manually, at around 652 A (set current) the reading current started going down (639.5 A)
Autoramp is set to -2 A each 10s to 0 A
The tantalum boat deformed and the graphite cartridge rim broke |
Friday, March 13, 2020, 14:21, Darwin Ortiz Rosales, SiC, 42218-8 , HP-SIS, Done, Conditioning of SiC discs (sintering) (RUSH)
|
Friday, March 13, 2020, 13:52
Total number of foils: 493
Total length packed 17.4 cm
container has 3 Ta heat shields.
No endcaps inserted to facilitate out-gassing
Two TaC coated Ta wire springs inserted at both ends.
Initially to ramp TGHT and TBHT to 50A at 1A/min
Then heat manually to OMEGA ~1400 C , ramping TGHT manually and automatically to reach 530A A (Omega slope set = 0.990)
Then temperature = 1800 (C using slope 1.08 at after 1700C manually and automatically ramp to 700A then TGHT will be tapped up accordingly to reach desired Temp).
TBHT will be set fixed at 230 A (max). TBHT heated manually and automatically to max.
Good vac at 3.00 e -5 Torr
Bad vac at 5.00 e-5 Torr
Evaluation discs not included because no space.
Total Green disc mass measured = 58.78 g
Friday, March 13, 2020, 14:22
Container loaded and pressuring down started without any pump issues.
Friday, March 13, 2020, 23:26
IGP1= 9.1e-07 Torr
Start auto tap at .25A/min to 50A on both TBHT and TGHT
Saturday, March 14, 2020, 07:09
IGP1=6.9e-6 Torr
TGHT = 49.1 A, 0.58V
TBHT = 49.2A, .49V
Continue ramp to 80 A on both heaters at .0.25A/min (good vacuum 3.0 e-04 Torr, bad vaccum 5.0 e-04 Torr
Saturday, March 14, 2020, 08:22
IGP1=6.8 e-05 Torr
Pressure spike TGHT =63.7 A, 0.77 V; TBHT = 60.0 A , 0.62 V
Aborted ramp alow to stabilize (Tapped TBHT to 63.8 A
Saturday, March 14, 2020, 12:16
IGP1= 8.1e-05 Torr
start autoramp at 0.25A/min
Saturday, March 14, 2020, 17:47
IGP1= 2.9e-05 Torr
TGHT= 78.4A, 1.0 V
TBHT = 79.4A, .88 V
manual and automatic tap up to 740A TGHT and 230A TBHT then tap manually to 1800 C (mostly at .075 A/min and increasing to 1A /min as pressure stabilizes)
Sunday, March 15, 2020, 22:40
OMEGA = 1711 C
TGHT = 784,6 A, 12.9V (readback)
TBHT = 232 A, 3.5 V
Tap TGHT to 800 A readback set to 815A
Sunday, March 15, 2020, 23:20
OMEGA =1801 C
TGHT = 799.2 A, 13.3 V, TBHT = 232.9, 3.6V
Start gradual tap-down as temperature rising (1810 C at end of this note)
Sunday, March 15, 2020, 23:49
OMEGAA = 1818 C
TGHT = 769.9A, 12.6 V; TBHT = 232.9 A, 3.6 V
Temperature dropping tapped back up to 799 A on TGHT read back (set to 815 A)
Monday, March 16, 2020, 04:10
OMEGA = 1395 C (not reliable)
TGHT = 799.2 A, 13.2 V
TBHT = 232.9 A, 3.6 V
IGP1 = 2.2 e-06 Torr
Initiate cooling at -1.5 A/min on TGHT to 600A (at 600 A increase cooling rate to 3 A/min ; at 300 A increase cooling to 4 A/min and start TBHT cooling at 1 A/min; at `200 A on TGHT increase cooling to 4 A/min and TBHT 2 A/min)
Monday, March 16, 2020, 09:43
TGHT = 0 A , 0.02V
TBHT = 53,2 A, .56 V (increase cooling to 4 A/min)
IGP1= 1.12e-07 Torr
Monday, March 16, 2020, 10:37
IGP1= 9.5 e -8 Torr
TGHT and TBHT = 0A, 0V
Will unload container
Monday, March 16, 2020, 12:40
Ten discs removed for evaluation (6 from left side and 4 from right side)
two graphite discs placed at each end as well as two TaC coated and sintered end-caps
total length after sintering = 17.8 cm
|
Tuesday, March 10, 2020, 09:34, Darwin Ortiz Rosales, Empty, 42218-8, HP-SIS, Done, TaC coating/sintering
|
Monday, March 9, 2020, 03:15
Container coated with TaC and wrapped with 3 Ta heat shields.
Desired temperature= 1900 C, Omega Slope set = 0.990, Auto TGHT at 0.2A/min to reach 400A, TGHT will be tapped up accordingly to reach desired Temp.
TBHT will be set fixed at 230 A (max).
Good vac at 3.00e -5 Torr
Bad vac at 5.00e-5 Torr
Chamber pump down
Tuesday, March 10, 2020, 09:17
Starting manual ramp to 50 A @ approximately 2A/min
IGP1 = 3.73e-7 Torr after opening water line pressure slowly incresed to 4.4e-7 Torr
TBHT also has Chiller interlock reached out to controls for removal.
Tuesday, March 10, 2020, 10:47
Chiller Interlock removed for TBHT. Started manual ramp to 50A @ approximately 2A/min
Tuesday, March 10, 2020, 11:15
allowing to stabilize at 50A on TGHT and TBHT
IGP1= 7.9 e=7 Torr and trending up
Tuesday, March 10, 2020, 12:09
Pressure on IGP1 spiked. Allowing to stabilize.
Tuesday, March 10, 2020, 14:36: Stopped By to check. Vacuum @ 3.02e-03T. Turbo pump appears to have tripped. Shut off Both PS. Prepare to vent. - Aaron S.
Tuesday, March 10, 2020, 14:48: Tightened all fittings (Just in case). HS side & HS waterline at the feed through. Roughing.
Tuesday, March 10, 2020, 15:06: TP1 @ 38KRPM 1.34e-04T & dropping. TGHT & TBHT PS on. Monitor before heating. -AS
Wednesday, March 11, 2020, 06:25: Vacuum @ 3.39e-07T. TGHT / TBHT PS on. - AS
Wednesday, March 11, 2020, 06:26: Manually tapped up TGHT / TBHT to 10 / 10 A. Ok.
Wednesday, March 11, 2020, 06:28: Auto-ramping TGHT / TBHT @ 4 A per min to 50 / 50 A.
Wednesday, March 11, 2020, 07:07: Vacuum @ 3.64e-07T. TGHT / TBHT @ 50 A. All appears stable. - AS
Wednesday, March 11, 2020, 07:036
Started autoramp at 2 A/min
IGP1= 3.6e-7 Torr
Wednesday, March 11, 2020, 08:06
TGHT=10 5A, 1.3 V TBHT = 105 A, 1.2 V
pressure rising fast; manual ramp down to 95A on both TGHT and TBHT
Wednesday, March 11, 2020, 09:54
IGP1= 4.7e-6 Torr; TGHT = 93.1 A, 1.2 V; TBHT = 95.1 A, 1.1 V
start autoramp at 1A/min (0.5 A/30s)
IGP1= 1.28e-5 Torr
TGHT = 108.3 A, 1.44 V
TBHT = 110 A, 1.29 V
Stop autoramp
Wednesday, March 11, 2020, 10:25
IGP1= 5.9e-5 Torr
manually tapped TGHT and TBHT set-current to 105 A respectively.
pressure dropping.
Wednesday, March 11, 2020, 11:18
IGP1=8.0e-06 Torr
manually ramp to set-current 115 A for both TGHT and TBHT at approximately 2A/ min
allow to stabilize before proceeding
Wednesday, March 11, 2020, 12:12
IGP1=7.02e-6 Torr
TGHT = 112.7 A, 1.5 V
TBHT = 114.6 A, 1.4 V
Auto-ramping at 1A/min TGHT to 430 A and TBHT top 230A
Wednesday, March 11, 2020, 18:45
IGP1= 1.2 e-06 Torr
TGHT=421.8 A, 6.2 V
TBHT = 231.9 A, 3.1 V
auto-ramp TGHT at 1A/min to set-current 530A
Wednesday, March 11, 2020, 23:08
IGP1= 1.3e-6 Torr
TGHT= 519.9 A, 7.87V
TBHT = 232.0 A, 3.1 V
start autoramp TGHT to 600A at 1A/min
Wednesday, March 11, 2020, 23:36
IGP1= 1.6e-6 Torr
TGHT = 542.9 A, 8.2V
TBHT = 232.9 A, 3.1V
Set autoramp to 750A on TGHT at 0.5 A/min
Thursday, March 12, 2020, 06:55
The Voltage set on TGHT was too low so current had not increased
IGP1= 1.5e-6 Torr
TGHT = 640 A, 10V
TBHT 232/9A, 3.1V
Oncrease TGHT voltage set to 14.5 and start autoramp at 3A/min to 750 A
Thursday, March 12, 2020, 7:43
TGHT = 735.7 A, 11.8V
OMEGA = 1595C
Auto -ramp set to 780 A for TGHT
Thursday, March 12, 2020, 7:58
OMEGA = 1655 C
TGHT set to 800 A at 3A/min
Thursday, March 12, 2020, 9:42
OMEGA = 1704 C
TGHT = 789.5 A, 13.0 V
Manual tap up to 837 A set on TGHT and 821 A readback
Thursday, March 12, 2020, 10:00
TGHT readback = 821.0 A, 13.7 V
OMEGA = 1744 C
TBHT same as previous entry.
Thursday, March 12, 2020, 10:35
Tapped up TGHT to 832.6 A, 13.8 V
OMEGA = 1759 C
TBHT = 232.9 A, 3.6 V
Will not tap further.
Thursday, March 12, 2020, 13:22
IGP1 = 5.0 e-06 Torr (stable)
TGHT = 832.7 A readback (849 A set), 13.7V
TBHT = 232.9 A, 3.6 V
OMEGA = 1758 C
Start cooling at TGHT 3A/min
Thursday, March 12, 2020, 14:08
IGP1= 1.32e-06 Torr
TGHT = 706 A, 11.0 V
TBHT = same as previous
OMEGA = 1583C
Start cooling TBHT at 1A/min continue cooling TGHT at 3A/min
Friday, March 13, 2020, 08:18
IGP1= 3.9e-8 Torr
Will unload sintered container
|
Wednesday, March 04, 2020, 14:33, Aaron Schmidt, , , , Maintenance, PS swap out
|
The TGHT PS was found to be defective.
It was uninstalled w/ Joel S: I2020-02-28-2.
It was replaced with the conditioning station PS & connected. The chiller is not required and has been unplugged.
Wednesday, March 04, 2020, 14:00. Controls Involved (PS still locked out via main breaker)
Wednesday, March 04, 2020, 14:31: Water supplies opened. All ok except Chiller (Disconnected from PS, but not the supply/return, do not open Chiller lines)
Controls work ongoing.
Thursday, March 05, 2020 (Darwin)
Gelo finished installation of the other power supply S:_____________________.
It was tested and proved to be operational and epics controlled. Tested up to 60A
Chiller interlock was removed as it is no longer needed.
Will wait for Aaron to swap FEBIAD assembly in EVAP 2.
|
Tuesday, December 03, 2019, 08:24, Aaron Schmidt, , , LP-FEBIAD, In progress, Temperature mapping.
|
Tuesday, December 03, 2019, 08:15: Waterlines opened. Vacuum ok @ 4.06e-07T
Tuesday, December 03, 2019, 08:23: Unable to start due to flow trip? PS off.
Tuesday, December 03, 2019, 08:25: Turbo & Vac off.
Tuesday, December 03, 2019, 08:51: Vented. Investigate. Install outer shields. Loose wire found on exterior paddle. Trip gone. Roughing.
Tuesday, December 03, 2019, 09:03: Turbo pump on.
Tuesday, December 03, 2019, 09:12: PS on. Vacuum @ 4.46e-05T and dropping.
Wednesday, December 04, 2019, 10:21: Manually tapped up the TGHT / TBHT to 35 / 10 A.
Wednesday, December 04, 2019, 10:22: Auto-ramping TGHT / TBHT to 300 / 150 A @ 2 A per min.
FM
Wednesday, December 04, 2019, 13:48: Auto-ramping TGHT / TBHT to 350 / 175 A @ 2 A per min.
Wednesday, December 04, 2019, 14:20: Auto-ramping TGHT / TBHT to 400/ 190 A @ 2 A per min.
Thursday, December 05, 2019, 10:58: Checking the striptool, approximately 30 minutes ago there was an oscillatory behaviour on the TGHT power. It went down to 0 in a very short time.
Temperature measurements were recorded and indicate a 70C difference from before the event.
Thursday, December 05, 2019, 15:08: Auto-ramping TGHT / TBHT to 450/ 230A @ 2 A per min.
Thursday, December 05, 2019, 19:05: Checking the striptool, at around 6 pm the TGHT power supply trip and didn't come back.
Thursday, December 05, 2019, 19:06: Drop in temperature indicates the target stop glowing.
Thursday, December 05, 2019, 19:07> Turning off power supply on EPICS and setting the slider to 0A.
I will ramp up TGHT in the morning while in the lab.
Friday, December 06, 2019, 14:55: Ramping down TBHT to 0A @ 2A/min
Tuesday, December 10, 2019, 09:11: Manually tapped up the TGHT / TBHT to 35 / 10 A
Tuesday, December 10, 2019, 09:12: Auto-ramping TGHT / TBHT to 400/ 230A @ 2 A per min.
Aborted |
Tuesday, November 26, 2019, 15:21, Darwin Ortiz Rosales, SiC, 42464-3, HP-FEBIAD, Done, Conditioning of SiC discs (sintering) (RUSH)
|
Tuesday, November 26, 2019, 14:53
Total number of foils: 504
Total length packed 17.4 cm
container has 3 Ta heat shields.
No endcaps inserted to facilitate out-gassing
Two TaC coated Ta wire springs inserted at either end.
Initially to ramp TGHT and TBHT to 50A at 1A/min
Then heat manually to OMEGA ~1400 C , ramping TGHT manually and automatically to reach 530A A (Omega slope set = 0.990)
Then temperature= (Correected to 1800C) 1900 C, Omega Slope set = 0.990, manually and automatically ramp to 700A, TGHT will be tapped up accordingly to reach desired Temp.
TBHT will be set fixed at 230 A (max). TBHT heated manually and automatically to max.
Good vac at 3.00 e -5 Torr
Bad vac at 5.00 e-5 Torr
System experienced some vacuum issues due to cooling water leak in a heatshield line.
Evaluation discs not included because no space.
Total Green disc mass measured = 58.250 g
Tuesday, November 26, 2019, 15:00
IGP1= 7.4e-06 Torr. No leak issues found after last fix (Anders will add details).
Tuesday, November 26, 2019, 15:33
TGHT= 52.7A, .22V TBHT= 49.3A, .52V
IGP1= 7.202 e-06 Torr (trending up so will allow to stabilize).
Wednesday, November 27, 2019, 06:09
left with autoramp waiting for vac to drop but no advance overnight.
Pressure did not seem to drop back below 3e-5 Torr magnitude, therefore not much advance in current ramp.
Thursday, November 28, 2019, 11:15
Continued ramping manually
OMEGA = 1429 C (0.99 slope), TGHT = 542A, 7.8V
With slope = 1.08 OMEGA = 1724 C, therefore staying at 0.99 slope
TaC coating sintering plot suggests 753A to reach 1800C (See attachment 1)
Windows a little bit coated but not enough to disturb laser.
Thursday, November 28, 2019, 12:17
TGHT =753A, 11.8V since 12:00 noon.
TBHT= 233.4A, 3.3V
OMEGA= 1735 C (0.99 slope)
Thursday, November 28, 2019, 13:01
OMEGA = 1860C (1.08 slope)
Thursday, November 28, 2019, 14:38
OMEGA temperature began to creep up to ~1880. Tapped TGHT current down to 733.5A, 11.4V
Thursday, November 28, 2019, 15:12
Checked windows and no significant additional buildup of obstructive material.
Temperature creeping up again. Tap down TGHT current to 729 A, 11.2 V
OMEGA = 1870C at slope 1.08
Thursday, November 28, 2019, 16:03
Temperature increase to 1880C
Tap down TGHT current to 715A, 10.9V
OMEGA= 1870 C (slope = 1.08)
Thursday, November 28, 2019, 16:22
Temperature creep to 1880 C
Tap down TGHT to 700A, 10.8V
OMEGA= 1845C
IGP1=2.2e-06 Torr
Thursday, November 28, 2019, 16:37
IGP1= 1.9e-06 Torr
OMEGA = 1850C (1.08 slope)
TGHT = 692A, 10.5V TBHT= 233A, 3.2V
Initiating pressure ramp at -2A/min on TGHT and -1A/min on TBHT
Thursday, November 28, 2019, 16:45
IGP1= 1.28e-06 Torr
OMEGA= 1770 C (1.08 slope)
TGHT = 650A, 9.8V
ramp TGHT at -3.5A/min maintain TBHT at -1A/m in
Thursday, November 28, 2019, 17:11
IGP1= 1.14e-06 Torr
OMEGA = 1730 C (1.08 slope)
ramp TGHT at -5A/min maintain TBHT at -1A/m
Thursday, November 28, 2019, 17:20
IGP1- 8.9e-07 Torr
OMEGA=1636C
ramp TGHT at -6A/min maintain TBHT at -1A/min
Thursday, November 28, 2019, 17:34
IGP1= 7e-07 Torr
OMEGA= 1500 C (1.08 slope)
ramp TGHT at -8A/min maintain TBHT at -1A/min
TBHT = 183A
OMEGA 1180C
TGHT =300 A
TBHT = 155A
Initiated -15A/min TGHT and -4A/min TBHT
IGP1= 5.2e-07 Torr
OMEGA below 1000C
begin manual tapdown
Thursday, November 28, 2019, 19:42
Target was dismounted after cooling. Two graphite discs and end caps inserted.
|
Wednesday, November 27, 2019, 17:45, John Wong, SiC, 42464-3, HP-FEBIAD, Done, Conditioning of SiC discs (sintering) (RUSH)
|
Darwin Ortiz Rosales wrote: |
Tuesday, November 26, 2019, 14:53
Total number of foils: 504
Total length packed 17.4 cm
container has 3 Ta heat shields.
No endcaps inserted to facilitate out-gassing
Two TaC coated Ta wire springs inserted at either end.
Initially to ramp TGHT and TBHT to 50A at 1A/min
Then heat manually to OMEGA ~1400 C , ramping TGHT manually and automatically to reach 530A A (Omega slope set = 0.990)
Then temperature= 1900 C (Correction = 1800 C, NOT 1900 - JW), Omega Slope set = 0.990 (use 1.08, check temp, JW), manually and automatically ramp to 700A (check temp to see if it's matching with the 1.08 slope), TGHT will be tapped up accordingly to reach desired Temp.
TBHT will be set fixed at 230 A (max). TBHT heated manually and automatically to max.
Good vac at 3.00 e -5 Torr
Bad vac at 5.00 e-5 Torr
System experienced some vacuum issues due to cooling water leak in a heatshield line.
Evaluation discs not included because no space.
Total Green disc mass measured = 58.250 g
Tuesday, November 26, 2019, 15:00
IGP1= 7.4e-06 Torr. No leak issues found after last fix (Anders will add details).
Tuesday, November 26, 2019, 15:33
TGHT= 52.7A, .22V TBHT= 49.3A, .52V
IGP1= 7.202 e-06 Torr (trending up so will allow to stabilize).
|
Wednesday, November 27, 2019, 17:44
I'll take over from here to step up the target heater, and I'll coordinate it with Darwin.
Wednesday, November 27, 2019, 20:36
Note: Sintering temp should be at 1800 C, NOT 1900. Use Omega slope 1.08 and check temperature. Correction made on elog #471.
Continue to step up TGHT and TBHT, keeping vacuum below 1.5 e-5 Torr.
Thursday, November 28, 2019, 03:06
TGHT reached to 400A/5.29V, TBHT at 230A/3.13V.
Vacuum coming down from 1.3 e-5 Torr.
OMEGA = 1105 C (slope at 0.99).
Instructions for Darwin:
1. Confirm temperature - check the temp plot from the TaC coating step.
2. Change OMEGA slop to 1.08 - check to see if this matches the temp plot. If not, bring it back to 0.99.
3. Continue to step up TGHT, check temp at 1400C (change slop 1.08 and check), 1500 C, 1600 C (check windows for coating - if any coating, then OMEGA is no longer useful hereon)
4. Use the temp plot and continue to tap up TGHT to reach 1800 C and hold it for at least 4 hours or until the vacuum goes below 1 e-6 Torr then proceed with cooling down.
5. Use the auto cooling program for TGHT (-2A/min) and TBHT (-1A/min)
Note: For ramping up TGHT, keep vacuum below 1.5 e-4 Torr and keep tapping up to reach 1800 C. Above 1100 C, this should be a quick step to get to 1800 C; should take < 2 hrs to get there.
See the striptool or the attachment below to see how I did it.
Once the chamber is cool down, take out a few samples for SEM analysis.
Good luck!
|
Tuesday, November 26, 2019, 15:43, Anders Mjos, SiC, 42464-3, HP-FEBIAD, Problems resolved, Water to vacuum leak on heat shield line
|
This morning, the vacuum responded to shutting of the water of the heat shield circuit (leak rate without pumping leveling out). The vacuum chamber was vented and the heat shield with flexible lines was replaced with another heat shield with fixed lines. The chamber was again pumped down and water opened at ~150 mTorr to test the leak up rate without pumping. No leaks apparent, so continued pumping down with turbo pump. At a vacuum of about 1E-6 Torr the water was again supplied to the heat shield circuit and an increase in vacuum could be observed. Stopped the turbo pump and prepared to vent. Two new heat shield lines were brazed in the machine shop and fitted by Maico after lunch. During this time one of the old lines (from heat shield to feedthrough in box) was leak tested and a leak found at a location just above the VCR. The line had been twisted and due to the twist developed a leak. With the two lines replaced, the vacuum was pumped down again and water could be supplied without any increase in vacuum pressure at 1E-6 Torr. To facilitate the new copper tubing, the restraining bracket for the heat shield VCRs was not mounted. It will have to be fitted later. Until then, please contact Anders for help in removing the heat shield to prevent any damage to the new lines. |
Monday, November 25, 2019, 11:35, Aaron Schmidt, , , , In progress, Flex - line HS installed
|
Leak noted on previous TaC sintering on HP FEBIAD # 42464-3.
Swapped out gaskets on HS flex line a re-tightened.
Monday, November 25, 2019, 11:31: Roughing.
Monday, November 25, 2019, 11:42: Turbo pump on.
Monday, November 25, 2019, 13:38: Vacuum @ 7.29e-06T.
Monday, November 25, 2019, 13:42: Waterlines opened. Vacuum slowly climbed to 7.57e-06T. Waterlines closed / purged.
Monday, November 25, 2019, 13:47: Vacuum @ 6.83e-06T.
Monday, November 25, 2019, 13:50: Waterlines opened. Vacuum gradually climbed again. Waterlines closed / purged.
Monday, November 25, 2019, 13:51: Turbo pump off.
Monday, November 25, 2019, 14:41: Vent. Check seals (All on HS line).
Monday, November 25, 2019, 14:48: Roughing.
Monday, November 25, 2019, 15:06: Vacuum @ 1.22e-04T. Waterlines opened. Vacuum continued to pump down steadily to 8.86e-05T and dropping.
Monday, November 25, 2019, 15:07: Turbo pump off. |
Saturday, November 23, 2019, 14:03, Darwin Ortiz Rosales, TaC, 42464-3, HP-FEBIAD, Done, TaC coating/sintering
|
12.3
Saturday, November 23, 2019, 14:00
Container coated with TaC and wrapped with 3 Ta heat shields.
Desired temperature= 1900 C, Omega Slope set = 0.990, Auto TGHT at 0.2A/min to reach 400A, TGHT will be tapped up accordingly to reach desired Temp.
TBHT will be set fixed at 230 A (max).
Good vac at 3.00e -5 Torr
Bad vac at 5.00e-5 Torr
Chamber pump down was started on Friday November 22; however.
No leaks were observed when turning water lines on.
IGP1= 4.6e-07 Torr
Saturday, November 23, 2019, 15:30
autoramp at 0.5A /min up to 50A for both TGHT and TBHT and maintained for 1 hour.
Saturday, November 23, 2019, 16:15
IGP1= 1.1e-06 Torr
Auto Ramp to 450 A on THGT and 230A on TBHT at 0.5A/min
Saturday, November 23, 2019, 23:44
IGP1= 5.2e-06 Torr
TGHT = 248A, 2.9V TBHT= 233A 2.9V
Increased ramp step to 1A/min to 620 A
Sunday, November 24, 2019, 00:14
IGP1=1.9e-06 Torr
TGHT = 274.3, 3.3V TBHT= 233A, 2.9V
Sunday, November 24, 2019, 07:33
IGP1=3.2e-06 Torr
OMEGA= 1490C
TGHT = 619 A, 9.1V TBHT=233A, 2.9V
Continue ramping THGT at 1A/min to 700 A
Sunday, November 24, 2019, 10:05
IGP1= 2.1 e-05 Torr
OMEGA= 1676 C
TGHT= 700A, 10.6V TBHT= 233A, 2.0V
Start autoramp to 780A as per regression in attachment
Sunday, November 24, 2019, 13:22
Autoramp to 795A for TGHT
Sunday, November 24, 2019, 21:16
OMEGA= 1854 C
TGHT= 789.6A, 12.27V TBHT= 233.A, 2.9V
IGP1= 2.0e-05
Will allow pressure to stabilize lower.
Sunday, November 24, 2019, 22:16
TGHTT= 789.6A, 12.3V TBHT=233.3A, 2.9V
OMEGA=1855C
IGP1 = 6.9e-06Torr
Start cooling TGHT at 2A/min and TBHT at 1A/min |
Friday, November 22, 2019, 18:32, Fernando Maldonado & Marla Cervantes , TaC, , HP-FEBIAD, In progress, TaC coating/sintering
|
Friday, November 22, 2019, 18:18:
Friday, November 22, 2019, 18:18: Roughing
Friday, November 22, 2019, 18:23: Turbo on .
Friday, November 22, 2019, 18:32: Turbo at speed
|
Thursday, November 21, 2019, 08:10, Aaron Schmidt, SiC, , HP-FEBIAD, In progress, Temperature mapping.
|
Thursday, November 21, 2019, 08:09: PS on. Leak issue resolved (Evap 2 Elog 466). Vacuum @ 4.10e-07T.
Thursday, November 21, 2019, 08:15: Auto-ramping TGHT / TBHT @ 2 A per min to 300 / 150 A. |
Friday, November 15, 2019, 13:26, Aaron Schmidt, SiC, , HP-FEBIAD, Problems resolved, Temp map testing - 1. (Leak issue)
|
HS 42752-5 - Setup for Temperature mapping.
Friday, November 15, 2019, 13:26: Roughing.
Friday, November 15, 2019, 13:36: Turbo pump on.
Monday, November 18, 2019, 07:46: Waterlines opened. Vacuum ok @ 3.56e-07T.
Monday, November 18, 2019, 07:48: PS on.
Monday, November 18, 2019, 09:21: PS off. Vacuum slowly spiked to 1.23e-06T. Indicative of a small water leak.
Monday, November 18, 2019, 09:24: HS waterlines purged. vacuum dropped to 5.54e-07T.
Monday, November 18, 2019, 09:27: Valves closed. TP off. BP off.
Monday, November 18, 2019, 10:27: Venting.
Monday, November 18, 2019, 11:06: Gaskets checked / replaced. Roughing.
Monday, November 18, 2019, 11:14: turbo pump on.
Monday, November 18, 2019, 14:19: Waterlines opened.
Monday, November 18, 2019, 14:23: Response on vacuum. Leak is still present & a higher rate (Has an immediate response). Turbos off.
Monday, November 18, 2019, 14:28: Venting.
Monday, November 18, 2019, 14:49: turbo pump on.
Tuesday, November 19, 2019, 07:07: Waterlines opened. Leak is present. Turbo pump off.
Tuesday, November 19, 2019, 11:24: After venting, changed 1 gasket. Setup LD & completed a leak check with the lines pressurized to 75 PSI of He.
Tuesday, November 19, 2019, 11:25: Roughing.
Tuesday, November 19, 2019, 11:33: Turbo pump on.
Wednesday, November 20, 2019, 08:59: Waterlines opened. Leak is present. Turbo pump off.
Wednesday, November 20, 2019, 11:26: FEBIAD Removed. U-Line installed to check Evap 2 Connection. FEBIAD examined outside.
Wednesday, November 20, 2019, 11:34: Turbo pump on.
Wednesday, November 20, 2019, 13:05: HPA off (Was running through HS line still. Vac @ 5.54e-06T).
Wednesday, November 20, 2019, 13:07: Open waterline. Vacuum @ 3.88e-06T & dropping steadily.
Wednesday, November 20, 2019, 13:12: Vacuum @ 3.69e-06T & dropping. No leak detected via Vac.
Wednesday, November 20, 2019, 13:14: Waterline Closed / purged. Turbo pumps off.
Wednesday, November 20, 2019, 13:58: Turbo pump on.
Wednesday, November 20, 2019, 13:50: Cleaned seal / FEBIAD re-installed. Roughing.
Thursday, November 21, 2019, 08:06: Waterlines opened. Vacuum ok @ 4.10e-07T.
Notes:
1) The FEBIAD left cooling line was the culprit for the leaks. A fine copper build up was noted on the gasket / sealing face. Images included.
2) Evap 2 was leak checked separately as well & is OK. |
Monday, November 04, 2019, 14:25, Darwin Ortiz Rosales, Endcaps, 40282-4, TARGET BOAT, Done,
|
Monday, November 04, 2019, 14:19
Each endcap is separated with a disc of graphite foil and rolled into packs one pack of 4 and one pack of 8 within a foil envelope in a target boat.
There are also 3 coated springs interspersed.
The boat is wrapped with 3-layers of Ta heatshields.
Chamber pumped down overnight.
OMEGA slope = 0.99
Will Tap TGHT up to 40 A then autoramp to 400A at 1A/min.
Final desired temperature on OMEGA (tap)= 1800C
Tuesday, November 05, 2019, 11:30
IGP1 = 9.6e-7 Torr
Autoramp TGHT to 40A at 1A/min
Tuesday, November 05, 2019, 11:44
IGP1= 2.6e-06 Torr
TGHT = 40.8 A, 0.37V
Will leave at 40 A for 1 hour
Tuesday, November 05, 2019, 12:39
IGP1=2.5e-6 Torr
TGHT =40.0A, .33V
Start ramping TGHT to 400A at 0.1A/min
Wednesday, November 06, 2019, 09:32
IGP1=7.8e-7 Torr
TGHT = 168.4A, 2.38V
increase ramp speed to 1A/min
Wednesday, November 06, 2019, 14:07
IGP1= 2.34e-6 Torr
TGHT=400.0 A, 6.98V
set TGHT autoramp to 460A @ 1A/min aiming for 1850C (see attached plot)
Wednesday, November 06, 2019, 15:18
OMEGA = 1776 C
TGHT = 460.0A, 8.52V
IGP1= 4.7e-6 Torr
Starting manual tap up to 1810C
Wednesday, November 06, 2019, 15:36
OMEGA=1810 C
TGHT = 468.8A, 8.74V
IGP1=4.14e-6
Wednesday, November 06, 2019, 19:04
OMEGA=1822 C (has been between 1817-1824 C over 3.5 hours )
TGHT=468.8A, 8.67V
IGP1=1.9498e-06 Torr
Start TGHT ramp down at -2A/min
Thursday, November 07, 2019, 09:55
THGT = 0A, 0V overnight
IGP1= 3.2 e-07 Torr
Proceeding with unloading.
End caps looked good for online use.
|
Thursday, October 17, 2019, 13:53, Darwin Ortiz Rosales, TaC, 44062-3, LP-SIS, In progress, TaC coating/sintering
|
Thursday, October 17, 2019, 12:00
Ta tube was coated with TaC and wrapped with Ta heat-shields (3 layers)
Desired temperature= 1900 C (expected TGHT ~430 A), TBHT will be set fixed at 230A (max).
Evap 2 was pumped down on the previous night.
Good vacuum= 3.00 e-5 Torr
Bad vacuum = 5.00 e-5 Torr
Ramped TGHT and TBHT to 40A at 0.5A/min
Initial IGP1= 7.0 e-07 Torr
Thursday, October 17, 2019, 13:53
After pressure stabilization at 40A:
Autoramp TGHT and TBHT at 1A/min to 400A and 230A respectively.
Friday, October 18, 2019, 6:20
TGHT = 400A, 6.52V, TBHT= 233A, 4.1V
OMEGA = 1733C
Start autoramp to 430A on TGHT at 1A/min
Friday, October 18, 2019, 7:05
TGHT= 431A, 7.1V
TBHT= 233A, 4.1V
IGP1= 1.13e-06 Torr
OMEGA = 1828 C
Set autoramp to 465 at 1A/min
Friday, October 18, 2019, 11:13
TGHT = 465A, 7.8V, TBHT = 233A, 4.1V
OMEGA = 1865C
(Something is different with the heat dissipation on this target. Will leave at this current and start cooling at 1200 noon to avoid container strain)
Friday, October 18, 2019, 12:00
TGHT = 462.7A, 7.8V
TBHT= 233.4A, 4.1V
OMEGA = 1863C
IPG1= 1.02e-06 Torr
Commence cooling at -2A/min for TGHT and -1A/min for TBHT
Monday, October 21, 2019, 09:11
Pump down and dismount.
|
Tuesday, October 08, 2019, 14:16, Aaron Schmidt, SiC, , HP-FEBIAD, In progress, Temp measurements.
|
Tuesday, October 08, 2019, 14:14: Remove Flex line HS.
HS: 42752-1
Waterlines not open yet.
Tuesday, October 08, 2019, 14:15: roughing.
Tuesday, October 08, 2019, 14:24: Turbo pump on.
Tuesday, October 08, 2019, 14:32: TP @ speed.
Wednesday, October 09, 2019, 13:24
The initial pressure was 3.25e-7 Torr
The current was manually increased to 25 A on both TBHT and TGHT at a rate of 1 A each 30 s for both heaters.
Wednesday, October 09, 2019, 13:33
At 1 pm an additional ram was made to TGHT 350 A and TBHT 200 at same rate. |
Monday, October 07, 2019, 09:18, Darwin Ortiz Rosales, TaC, , TARGET BOAT, In progress, Sintering TaC coating on endcaps and springs
|
Friday, October 04, 2019, 11:37
Each endcap is separated with a disc of graphite foil and rolled into packs of 5 within a foil envelope in a target boat.
There are also 3 coated springs, one in between endcaps and two on either end
The boat is wrapped with 2-layers of Ta heatshields.
Chamber pumping down
OMEGA slope = 0.99
Will Tap TGHT up manually to 40 A then autoramp to 400A at 1A/min.
Final desired temperature on OMEGA (tap)= 1800C
Monday, October 07, 2019, 09:08
Sunday night heating started at 1A/ min on TGHT to 54 A
heating paused for 1 hour to allow IGP1 to equillibrate. Then restarted at 1A/min to 400A as planned.
This morning IGP1 = 1.3e-06 Torr
TGHT = 401A, 4.2V
OMEGA = 1550 C
Monday, October 07, 2019, 09:36
manually tapping to 1800 C
Monday, October 07, 2019, 14:09
Temperature @ ~1800 for 3.5 hours
TGHT= 495.4, 9.2 V
IGP1= 1.1e-06 Torr Pressure Steady there begin cooling
Cooling @ -2A/min
|
Thursday, October 03, 2019, 09:26, Darwin Ortiz Rosales, TaC, 44062-6, LP-SIS, Done, TaC coating/sintering
|
Thursday, October 03, 2019, 08:58
Ta tube was coated with TaC and wrapped with Ta heat-shields (3 layers)
Initial weight including heat-shields = 427 g
Desired temperature = 1900 C (expected TGHT ~430 A), TBHT will be set fixed at 230A (max).
Evap 2 was pumped down previous night.
IGP1= 7.81e-07 Torr
Manually tapping up to ~40A on both TGHT and TBHT at ~1A/min
Good vacuum = 3.00 e-5 Torr
Bad vacuum = 5.00 e-5 Torr
Thursday, October 03, 2019, 09:21
Manually tapped to 50A on TGHT and TBHT
Will allow pressure to stabilize and begin autoramp TGHT and TBHT at 1A/min to 400A and 230A respectively.
autoramp increments might be increased to 2A/min depending on stability of system.
Thursday, October 03, 2019, 10:00
TGHT = 51.6A, 0.36V
TBHT = 49.5A, 0.62V
IGP1=9.6e-7 Torr
Starting autoramp at 1A/min to a max of 400A for TGHT and 230A for TBHT. Will monitor and increase ramp increments to 2A/min if stable.
Thursday, October 03, 2019, 11:09
TGHT = 103A, TBHT=97A
IGP1=9.1e-06 Torr and dropping
Will increase autoramp increments to 2A/min
Thursday, October 03, 2019, 11:41
With TGHT = 148A, 1.9V and TBHT = 141A, 2.3V
IGP1= 7.9e-6 Torr
Autoramp was increased to 3A/min
Thursday, October 03, 2019, 13:45
TGHT=401A, 6.9V
TBHT=233A, 4.2V
IGP1= 1.14e-05Torr
OMEGA = 1874
begin manual ramp to 1900C
(Temperature dropping as pressure drops)
Thursday, October 03, 2019, 14:11
TGHT= 416A, 7.1V
TBHT=233A, 4.2V
OMEGA = 1900 C
IGP1= 6.9e-06 Torr and trending down
Thursday, October 03, 2019, 15:24
TGHT manually bumped to 421A, 7.2 V because temperature dropped slightly.
Thursday, October 03, 2019, 19:00
TGHT manually increased to 425A, 7.3V
Thursday, October 03, 2019, 19:12
TGHT = 424.9A, 7.3V
TBHT=233.2A, 4.1V
OMEGA= 1897 C
IGPA=1.45e-06 Torr
Starting ramp-down at -1A/min on TGHT and 0.5A/min on TBHT
Friday, October 04, 2019, 11:34
Container taken out.
|
Friday, September 27, 2019, 18:18, Marla Cervantes, Nb, , TARGET BOAT, Done, Conditioning NB samples for Edward
|
Wednesday, September 25, 2019, 18:06
Target boat with a layer of niobium foil on the bottom is used to heat up Nb samples to 1400 C for 4 hrs.
The niobium samples are wrapped in a Nb foil.
Boat is wrapped with 2 layers of Ta foil, careful to avoid touching samples.
Thursday, September 26, 2019, 18:10
The target assembly was exchange to a clean one e-log 459 and the Nb arrangement was loaded into evap2.
Friday, September 27, 2019, 18:13
HS water valves opened, no leaks detected.
Tapped up manually to 40 A.
IGP1 = 9.54e-7 Torr
Setting auto-ramp rate at 0.2 A/min to max setpoint of 100 A.
Vacuum stable.
Setting auto-ramp at 1 A/min to 300 A lead to ~1200 C.
Autoramping at 1 A/min to 400 A will stop at 1400 C.
Temperature reading is 1400 C at:
TGHT = 5.61 V, 345.656 A
The temperature reading went to 1408 C on Omega and 1417 C on Micron so the current was dropped to 342.537 A and 5.56 V
The temperature went to 1418 C on Omega and the current was dropped to 339.281 A
After 4 hours at 1400 C, the Nb was cooled down
The final pressure was 3.07e-7 Torr
The EVAP2 was vented with air and the Nb was removed. |
Thursday, September 26, 2019, 14:03, Aaron Schmidt, Nb, 41882-3, TARGET BOAT, In progress, HS swap & test Nb target
|
HS# 42752-7
Thursday, September 26, 2019, 13:46: Remove Flexible lines HS
Thursday, September 26, 2019, 14:03: Assy installed.
Friday, September 27, 2019, 07:07: Vacuum @ 1.16e-06T.
Friday, September 27, 2019, 07:09: Waterlines opened. Vacuum stable @ 1.15e-06T
Monday, September 30, 2019, 10:04: Remove Nb target & assy. Install flexible line HS. |
Tuesday, September 17, 2019, 13:25, Aaron Schmidt, , , LP-SIS, Problems resolved, Turbo pump / roughing troubleshoot.
|
Swapped out VCRs on HS to tray connection. (Right one felt slightly off)
Tuesday, September 17, 2019, 13:23: roughing.
Tuesday, September 17, 2019, 13:32: Turbo pump on.
Tuesday, September 17, 2019, 13:44: waterlines re-opened. No vacuum response. Ok. @ 7.90e-05T & dropping.
Wednesday, September 18, 2019, 08:05: Vacuum ok @ 6.87e-07T. Turbo pump off.
Wednesday, September 18, 2019, 08:21: Venting.
Pumped down again easy for Ta#59. Issue resolved. |
Monday, September 16, 2019, 14:50, Aaron Schmidt, Ta, 44062-5, LP-SIS, In progress, Conditioning Ta#59
|
Ta#59 LP-SIS target description:
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.025mm
Target density = 13.74 g/cm3
Target length = 3.4 cm
Total Mass = 46.7314 g [Incl foils + Ta wire on 6 packs]
Total mass w/ Target oven= 436 g (440 g w/ end caps)
Discs in target are arranged as follows: 1pack / 75singles / 1pack / 100singles / 2packs / 100singles / 1pack / 75singles / 1pack
End caps installed (not yet expanded). No Ta heat shield added.
Monday, September 16, 2019, 14:47: Roughing.
Monday, September 16, 2019, 14:55: Turbo pump on.
Monday, September 16, 2019, 15:04: Timed out. Open RV1
Monday, September 16, 2019, 15:05: Restart Turbo pump.
Monday, September 16, 2019, 15:14: Attempt stop / restart before timeout.
Monday, September 16, 2019, 15:21: Turbo pump unable to pass 4krpm. Close for re-attempt tomorrow am.
Tuesday, September 17, 2019, 12:33: Venting. Sort out pump down issues.
TBHT will be ramped up to 230A at 1.0A/min.
TGHT will be ramped up to 650A at 2.0A/min.
Final desired temperature = 1900C.
OMEGA slope = 0.98.
Wednesday, September 18, 2019, 08:50: Omega slope set to 0.98. Power supplies / sources on. vacuum@ 3.34e-05T & dropping.
Wednesday, September 18, 2019, 08:25: Roughing.
Wednesday, September 18, 2019, 08:34: Turbo pump on.
Wednesday, September 18, 2019, 10:22: TGHT manually to 40A. Vacuum @ 3.18e-06T.
Wednesday, September 18, 2019, 10:25: Auto-ramping TGHT / TBHT @ 2 / 1 A per min to 350 / 180 A.
Wednesday, September 18, 2019, 13:43: Vacuum @ 2.30e-06T. Temp @ 1120 deg C. TGHT / TBHT @ 350 / 180 A.
Wednesday, September 18, 2019, 13:45: Auto-ramping TGHT / TBHT @ 2 / 1 A per min to 550 / 215 A.
Thursday, September 19, 2019, 06:39: Vacuum @ 8.79e-07T. Temp @ 1722 deg C. TGHT / TBHT @ 550 / 215 A.
Thursday, September 19, 2019, 06:42: Auto-ramping TGHT / TBHT @ 2 / 1 A per min to 600 / 230 A.
Thursday, September 19, 2019, 08:18: Auto-ramping TGHT to 630A @ 2 A per min
Step up to desired temp
Thursday, September 19, 2019, 08:49: Vacuum @ 3.22e-06T. TGHT / TBHT 645 (642.7) / 230 (233.44) A. TGHT Voltage= 12.501V. Omega: 1902-1903 deg C. Desired temperature = 1900C reached.
Thursday, September 19, 2019, 14:17: Vacuum @ 1.45e-06T. Begin auto-cooling TGHT / TBHT @ -1 / -1 A per min.
Friday, September 20, 2019, 07:59: Turbo pump off. PS / Sources off.
Friday, September 20, 2019, 08:42: Venting. |
Wednesday, September 11, 2019, 15:16, Marla Cervantes, , 44062-4, LP-SIS, Done, TaC coated target container calibration/conditioning
|
Wednesday, September 11, 2019, 15:12
A target container coated with TaC elog 455 was loaded with an empty graphite cartridge and set it in the EVAP2
The system is currently pumping down.
The target container was wrapped with 3 new Ta heat shields.
The target container will be heated to 2000 C and the temperature will be held for 4 hours.
The autoramp was set to:
TGHT 1 A/min, 450 A
TBHT 0.5 A/min, to 230 A
At 500 A on the TGHT, 20 additional amps were programmed to increased at 1 A/min, however, the autoramp increased the current to 520 A without stepping (see figure A).
The final conditions were:
TGHT: 9.95 V, 565.59 A
TBHT: 4.18 V, 233.43 A
IGP1: 2.2 e-6 Torr
Friday, September 13, 2019, 11:16
After 4 hours the EVAP2 was cooled down
at a rate of TGHT 1 A/min and TBHT 0.5 A/min
The EVAP2 was vented with air.
|
Friday, September 06, 2019, 11:58, Darwin Ortiz Rosales, , 44062-4, LP-SIS, Done, TaC coating/sintering
|
Friday, September 06, 2019, 11:20
Container was coated with Tac and wrapped with 2 Ta heat shields.
Desired temp=1900 C, Omega slope set =0.990
Chamber pumped down over night and will be initially tapped manually to 40A for both TGHT and TBHT.
Subsequently, current will be automatically ramped up in increments of 1A/min to reach 400A for TGHT and 230A for TBHT.
Then TGHT will be manually tapped to target temperature and allow to stabilize for a minimum of 3 hours.
Good vac at 3.0e-5 Torr
Bad vac at 5.0e-5 Torr
Friday, September 06, 2019, 11:32
IEVAP2:IGP1=9.6e-7 Torr
Tapping to 40A (TGHT and TBHT).
Friday, September 06, 2019, 12:54
Start autoramp
1A/min TGHT and TBHT
IGP1=4.0e-06 Torr
Friday, September 06, 2019, 13:29
TGHT = 70A, TBHT=70A, pressure started to spike rapidly so aborted autoramp and lowered the current to 66A for both TGHT and TBHT.
pressure continued to rise so tapped current to 60A. A drop observed. Will allow to stabilize.
Friday, September 06, 2019, 14:06
IGP1=5.3e-06 Torr. Restart previous ramping.
At 66A paused ramping. IPG1= 1.0e-5 Torr
Friday, September 06, 2019, 15:44
IGP1=6.0e-6 Torr
Start modified autoramping: 0.4A/min for TGHT and TBHT. Will manually tap up in the morning, over ham and eggs.
Saturday, September 07, 2019, 10:52
Will tap up to 423 A on TGHT as per attachment #1 regression
IGP1= 1.13e-6 Torr
OMEGA = 1802 C
TGHT= 401.0 A, 6.84V
TBHT=233.6A, 4.1V
Saturday, September 07, 2019, 11:06
Tapped up TGHT to 438A
OMEGA= 1903C
Will monitor and adjust if necessary.
Saturday, September 07, 2019, 15:06
IGP1 = 1.17e-6 Torr
TGHT = 7.46 V, 439.3 A
TBHT = 4.13 V, 233.4 A
Autoramps
TGHT = -2 A/min, TBHT = -1 A/min
Monday, September 09, 2019, 16:34
The EVAP2 was vented and the target container was removed.
|
Wednesday, August 28, 2019, 05:59, Marla Cervantes, , 44062-2-SK, , Done, Graphite insert test
|
Wednesday, August 28, 2019, 06:00
A graphite insert (with conical caps) was loaded in tantalum tube
the Ta tube was wrapped with 3 tantalum foils,
a tantalum cap was inserted in one side of the Ta tube and sealed.
The tube was set in the EVAP2 and the furnace was pumped down.
IGP1 = 1.23e-6 Torr.
The current was tapped to 50 A
Autoramp was set to 1 A/min to 400 A.
Wednesday, August 28, 2019, 12:02
Autoramp reached 400 A
TGHT = 6.57 V, 404.4 A, IGP1=4.7e-6 Torr
Autoramp was set to 450 A at 1A/min
Wednesday, August 28, 2019, 12:48
Autoramp reached 450 A
TGHT =7.526 V, 450.188 A, IGP1=5.88e-6 Torr
Autoramp was set to 500 A at 1A/min
Wednesday, August 28, 2019, 13:40
Autoramp reached 500 A, temperature 1880 C
TGHT =8.79 V, 501.094A, IGP1=7.48-6 Torr
Autoramp was set to 540 A at 1A/min
Wednesday, August 28, 2019, 14:03
The autoramp was stopped at 520 A, because according to previous tests that current is enough to have 2000 C,
the temperature read was 1930 C
TGHT =9.23 V, 520.7 A, IGP1=7.8-6 Torr
Wednesday, August 28, 2019, 15:20
The autoramp was set to 540 A at 1A/min
When the ramp stopped the conditions were:
TGHT=9.59 V, 539.5 A, IGP1= 6.08e-6 Torr
Temperature= 1988 C
Manually tapped to 545 A the temperature reached 2000 C
Wednesday, August 28, 2019, 17:08
To keep the temperature at 2000 or less the current was decreased,
TGHT= 8.91 V, 445.125 A, IGP1=9.93e-7 Torr
Max temperature read: 2001 C
Min temperature read: 1996 C
Tuesday, September 03, 2019, 11:15
The tube was stable at 1950-1960 C during the weekend but today at around 6 am it had a drop in the current indicating mechanical failure
The autoramp was set to -2A/min to 0 A.
The tube will be examined and in case that it is not broken it will be set in the EVAP1 to continue heating it.
Monday, September 09, 2019, 16:35
The tube became brittle and broke. |
Tuesday, July 30, 2019, 15:42, Darwin Ortiz Rosales, ZrC, 43044-6, LP-SIS, Done, Sintering ZrC Discs
|
Tuesday, July 30, 2019, 15:33
ZrC backup Target 12.6 cm disc length, 465 g total weight (no springs and no analysis discs).
Total weight= 470 g.
20 Analysis discs weighing 2.368 g (10 at each end).
Two springs (one at each end).
OMEGA slope initially = 0.990 (was changed to 1.09 at higher Temperature as per eLog #434
Target is being pumped down.
Wednesday, July 31, 2019, 09:31
Desired temp = 1900 C, Auto ramping TGHT at 0.1 A/min to reach 400A then TGHT will be tapped up accordingly to reach desired temperature. (eLog 434)
TBHT will be set fixed at 230A (max). TBHT at 0.1 A/min to reach 230A.
Note: Initially both TGHT and TBHT will be ramped up at 0.3A/min up to 30A each.
IGP1= 1.35e-06 Torr
Good vac at 3.00-5 Torr
Bad vac at 5.0e-5 Torr.
Wednesday, July 31, 2019, 12:02
At 30A pressure was increasing a bit fast, therefore, the ramp was changed to increments of .1A every 120s (.05A/min).
Thursday, August 01, 2019, 08:42
TGHT = 54.7
TBHT = 54.3
IGP1 = 3.86e-5 Torr
Will changer heat ramp to .1A/min by changing wait interval to 60s
Tuesday, August 06, 2019, 07:14
OMEGA = 1212 C
TGHT = 344.7 A, 5.79 V
TBHT = 233 A, 4.17 V
IGP1 = 1.05 e-06 Torr
Autoramping to 400A at increments of 0.1A/min
Tuesday, August 06, 2019, 09:50
OMEGA = 1233 C
TGHT = 360 A, 6.05 V
TBHT = 233 A, 4.18 V
IGP1 = 1.21 e-06 Torr
increasing autoramp increments to .5A/min
Tuesday, August 06, 2019, 12:27
OMEGA = 1356 C
TGHT = 400.6 A, 6.92 V
TBHT = 233.8 A, 4.20 V
IGP1 = 1.95 e-06 Torr
Autoramping to 430 A on TGHT at 0.5 A/min
Tuesday, August 06, 2019, 14:02
OMEGA = 1447 C
TGHT= 430.9 A, 7.66V
TBHT = 233.2A, 4.2 V
IGP1= 2.01e-06 Torr
Autoramping to 440 A on TGHT at 0.5 A/min
Wednesday, August 07, 2019, 09:10
OMEGA = 1548
TGHT = 441.56 A, 8.2 V
TBHT = 233.3 A, 4.2 V
IGP1 = 6.21e-07 Torr
Manually ramping up to 1900C @ 1A/min
Wednesday, August 07, 2019, 09:43
Changed OMEGA slope to 1.09 as per eLog #434
OMEGA reads 1773 C @ TGHT 451A, 8.4V
IGP1 = 7.02 e-07
Wednesday, August 07, 2019, 10:56
OMEGA = 1903 C
TGHT = 483.5 A, 9.2V
TBHT = 233.3 A, 4.3V
IGP1 = 1.7 e-06 Torr trending down
Wednesday, August 07, 2019, 11:40
OMEGA = 1914 C
TGHT = 483.5 A, 9.3V
TBHT = 233.3 A, 4.3V
IGP1 = 1.5 e-06 Torr trending down
Decrease TGHT current to 480.4 A
Wednesday, August 07, 2019, 13:04
OMEGA = 1918 C
TGHT = 480.3 A, 9.4V
TBHT = 233.3 A, 4.3V
IGP1 = 1.28e-06 Torr
Decrease TGHT current to 474.5 A
Wednesday, August 07, 2019, 13:26
OMEGA = 1904 C
TGHT = 474.8 A, 9.3V
TBHT = 233.3 A, 4.3V
IGP1 = 1.11e-06 Torr
Wednesday, August 07, 2019, 13:47
OMEGA = 1912 C
TGHT = 474.8 A, 9.3V
TBHT = 233.3 A, 4.3V
IGP1 = 1.10e-06 Torr
Decrease TGHT to 471.8 A
OMEGA temperature went down to 1904 C
Wednesday, August 07, 2019, 14:26
OMEGA = 1911 C
TGHT = 471.8 A, 9.3V
TBHT = 233.3 A, 4.3V
IGP1 = 1.00e-06 Torr
Decrease TGHT to 469.0 A
OMEGA temperature down to 1904C
Wednesday, August 07, 2019, 15:45
OMEGA = 1912 C
TGHT = 468.8.8 A, 9.2V
TBHT = 233.3 A, 4.3V
IGP1 = 9.2e-07 Torr
Decrease TGHT to 466.0 A
OMEGA temperature down to 1903C
Wednesday, August 07, 2019, 22:09
OMEGA = 1924 C
TGHT = 466.8. A, 9.3V
TBHT = 233.3 A, 4.3V
IGP1 = 7.6e-07 Torr
Cooling at 2A/min TGHT to 456.0 A, 9.0 V and 1A/min TBHT to 230.1 A, 4.2 V
OMEGA = 1900 C
Will allow Pressure to stabilize
Thursday, August 08, 2019, 06:54
OMEGA = 1919 C
TGHT = 456.9 A, 9.1V
TBHT = 230.3 A, 4.2 V
IGP1 =5.7e-07 Torr
Cooling at 2A/min TGHT and 1A/min TBHT
Thursday, August 08, 2019, 13:30
Target removed from Evap2. Awaiting inspection by John.
|
Monday, August 12, 2019, 15:55, John Wong, ZrC, 43044-6, LP-SIS, Done, Sintering ZrC Discs
|
Darwin Ortiz Rosales wrote:
|
Tuesday, July 30, 2019, 15:33
ZrC backup Target 12.6 cm disc length, 465 g total weight (no springs and no analysis discs).
Total weight= 470 g.
20 Analysis discs weighing 2.368 g (10 at each end).
Two springs (one at each end).
OMEGA slope initially = 0.990 (was changed to 1.09 at higher Temperature as per eLog #434
Target is being pumped down.
Wednesday, July 31, 2019, 09:31
Desired temp = 1900 C, Auto ramping TGHT at 0.1 A/min to reach 400A then TGHT will be tapped up accordingly to reach desired temperature. (eLog 434)
TBHT will be set fixed at 230A (max). TBHT at 0.1 A/min to reach 230A.
Note: Initially both TGHT and TBHT will be ramped up at 0.3A/min up to 30A each.
IGP1= 1.35e-06 Torr
Good vac at 3.00-5 Torr
Bad vac at 5.0e-5 Torr.
Wednesday, July 31, 2019, 12:02
At 30A pressure was increasing a bit fast, therefore, the ramp was changed to increments of .1A every 120s (.05A/min).
Thursday, August 01, 2019, 08:42
TGHT = 54.7
TBHT = 54.3
IGP1 = 3.86e-5 Torr
Will changer heat ramp to .1A/min by changing wait interval to 60s
Tuesday, August 06, 2019, 07:14
OMEGA = 1212 C
TGHT = 344.7 A, 5.79 V
TBHT = 233 A, 4.17 V
IGP1 = 1.05 e-06 Torr
Autoramping to 400A at increments of 0.1A/min
Tuesday, August 06, 2019, 09:50
OMEGA = 1233 C
TGHT = 360 A, 6.05 V
TBHT = 233 A, 4.18 V
IGP1 = 1.21 e-06 Torr
increasing autoramp increments to .5A/min
Tuesday, August 06, 2019, 12:27
OMEGA = 1356 C
TGHT = 400.6 A, 6.92 V
TBHT = 233.8 A, 4.20 V
IGP1 = 1.95 e-06 Torr
Autoramping to 430 A on TGHT at 0.5 A/min
Tuesday, August 06, 2019, 14:02
OMEGA = 1447 C
TGHT= 430.9 A, 7.66V
TBHT = 233.2A, 4.2 V
IGP1= 2.01e-06 Torr
Autoramping to 440 A on TGHT at 0.5 A/min
Wednesday, August 07, 2019, 09:10
OMEGA = 1548
TGHT = 441.56 A, 8.2 V
TBHT = 233.3 A, 4.2 V
IGP1 = 6.21e-07 Torr
Manually ramping up to 1900C @ 1A/min
Wednesday, August 07, 2019, 09:43
Changed OMEGA slope to 1.09 as per eLog #434
OMEGA reads 1773 C @ TGHT 451A, 8.4V
IGP1 = 7.02 e-07
Wednesday, August 07, 2019, 10:56
OMEGA = 1903 C
TGHT = 483.5 A, 9.2V
TBHT = 233.3 A, 4.3V
IGP1 = 1.7 e-06 Torr trending down
Wednesday, August 07, 2019, 11:40
OMEGA = 1914 C
TGHT = 483.5 A, 9.3V
TBHT = 233.3 A, 4.3V
IGP1 = 1.5 e-06 Torr trending down
Decrease TGHT current to 480.4 A
Wednesday, August 07, 2019, 13:04
OMEGA = 1918 C
TGHT = 480.3 A, 9.4V
TBHT = 233.3 A, 4.3V
IGP1 = 1.28e-06 Torr
Decrease TGHT current to 474.5 A
Wednesday, August 07, 2019, 13:26
OMEGA = 1904 C
TGHT = 474.8 A, 9.3V
TBHT = 233.3 A, 4.3V
IGP1 = 1.11e-06 Torr
Wednesday, August 07, 2019, 13:47
OMEGA = 1912 C
TGHT = 474.8 A, 9.3V
TBHT = 233.3 A, 4.3V
IGP1 = 1.10e-06 Torr
Decrease TGHT to 471.8 A
OMEGA temperature went down to 1904 C
Wednesday, August 07, 2019, 14:26
OMEGA = 1911 C
TGHT = 471.8 A, 9.3V
TBHT = 233.3 A, 4.3V
IGP1 = 1.00e-06 Torr
Decrease TGHT to 469.0 A
OMEGA temperature down to 1904C
Wednesday, August 07, 2019, 15:45
OMEGA = 1912 C
TGHT = 468.8.8 A, 9.2V
TBHT = 233.3 A, 4.3V
IGP1 = 9.2e-07 Torr
Decrease TGHT to 466.0 A
OMEGA temperature down to 1903C
Wednesday, August 07, 2019, 22:09
OMEGA = 1924 C
TGHT = 466.8. A, 9.3V
TBHT = 233.3 A, 4.3V
IGP1 = 7.6e-07 Torr
Cooling at 2A/min TGHT to 456.0 A, 9.0 V and 1A/min TBHT to 230.1 A, 4.2 V
OMEGA = 1900 C
Will allow Pressure to stabilize
Thursday, August 08, 2019, 06:54
OMEGA = 1919 C
TGHT = 456.9 A, 9.1V
TBHT = 230.3 A, 4.2 V
IGP1 =5.7e-07 Torr
Cooling at 2A/min TGHT and 1A/min TBHT
Thursday, August 08, 2019, 13:30
Target removed from Evap2. Awaiting inspection by John.
|
Monday, August 12, 2019, 15:45
Visual inspection on the target was performed today. See attachment for details.
Target container is slightly bent, and some visible crystallization on the container surface.
The discs are nicely packed with only a slight expansion in length was measured.
No clogging inside the container nor the ionizer tube.
Some sintered discs samples were collected and SEM will be perform later.
|
Wednesday, July 17, 2019, 11:13, Marla Cervantes, Nb, 40282-4, TARGET BOAT, Done, Annealing of RRR-Nb test samples
|
Wednesday, July 17, 2019, 10:57
Annealing of five RRR Nb samples following cold-working and resistance measurements. Used to validate computational annealing model developed for SRF studies. For more information contact Norman Muller, x6398.
Desired temperature 1025 C.
Five Nb samples wrapped with Nb foil were set on a tantalum boat (coated with TaC)
the tantalum boat was wrapped with two tantalum sheets.
The boat was installed in the EVAP2.
The initial vacuum was IGP1 = 1.26e-6 Torr.
Ramping rate 5 A/min to final current of 200 A.
Wednesday, July 17, 2019, 11:18
At 155 A, the ramping rate was changed to 1 A/min
Wednesday, July 17, 2019, 11:28
The ramping was stopped at 167 A.
Wednesday, July 17, 2019, 11:57
Conditions:
IGP1 = 1.65e-6 Torr
TGHT = 2.54 V, 174.46 A
Temperature ~ 950 C
Wednesday, July 17, 2019, 18:07
IGP1 = 1.16 e-6
TGHT = 3.18 V, 206.7 A
Temperature ~950 C
Cooling ramp 10 A/min
Vented with air
Suggestion for future annealing:
Use tantalum boat without TaC coating. |
Monday, June 24, 2019, 08:42, Darwin Ortiz Rosales, SiC, 42464-4, HP-FEBIAD, Done, Conditioning of BSiC discs
|
Monday, June 24, 2019, 08:24
Total number of foils: 484
Total mass in including container = 1495 grams
Total length packed 17.28 cm
container has 3 Ta heat shields.
No endcaps inserted to facilitate outgassing
Two TaC coated Ta wire springs inserted at either end.
Initially will heat via autoramp to OMEGA 1400 C , ramping TGHT at 0.1 A/min to reach 530A A (Omega slope set = 0.990)
Then temperature= (Correction to 1800C) 1900 C, Omega Slope set = 0.990, Auto TGHT at 0.2A/min to reach 700A, TGHT will be tapped up accordingly to reach desired Temp.
TBHT will be set fixed at 230 A (max). TBHT at 0.1 A/min.
Good vac at 3.00 e -5 Torr
Bad vac at 5.00 e-5 Torr
System was pumped down on Friday June 24th, 2019.
IGP1= 3.3 e-07 Torr
(EPICS was down this morning and came back up around 930 a.m.)
Will proceed to manually tap up TGHT and TBHT to 40A as soon as EPICS stability confirmed
Mondayy, June 24, 2019, 15:30
TBHT = 39 A, 0.4V
TGHT=40 A, 0.1V
IGP1= 4.3 e-06 Torr and trending down
Autoramp increments to 0.1 A/min , to 400A on TGHT and 230A on TBHT
Tuesday, June 25, 2019, 08:40
Current has only increased to 53 A and pressure limit reached. Lowered current back to 51 A on TGHT and TBHT. Waiting for pressure to stabilize.
Tuesday, June 25, 2019, 12:16
TGHT 51.3 A, 0.39 V
TBHT 51.1 A, 0.58 V
IGP1 = 1.91 e-05 Torr
Starting autoramp with increments to 0.1 A/min , to 400A on TGHT and 230A on TBHT
Saturday, June 29, 2019, 22:45
Autoramp increments for TGHT set to 0.2 A/min
IGP1=2.4 e-06 Torr
Sunday, June 30, 2019, 07:46
Autoramp incrementsTGHT set to 0.1 A/min to prevent pressure spike.
IGP1= 1.5 e-05 Torr
Sunday, June 30, 2019, 08:26
Set autoramp increments on TGHT back to 0.2 A/min
Sunday, June 30, 2019, 15:47
Set autoramp max on TGHT to 500 A
Sunday, June 30, 2019, 21:15
OMEGA = 1240C
TGHT= 465A, 7.0V
TBHT = 233A, 3.2V
IGP1= 1.6 e-05 Torr
Set autoramp max on TGHT to 600A
Monday, July 01, 2019, 09:48
OMEGA = 1605 C
TGHT = 599A, 9.7V
TBHT = 233A, 3.2V
IGP1= 1.3 e-06 Torr
Set autoramp max on TGHT to 650A
Monday, July 01, 2019, 18:21
OMEGA = 1630 C
TGHT = 650 A, 10.6V
TBHT = 233A, 3.2V
IGP1 = 9.7 e-07 Torr
Set utoramp max on TGHT to 700A
Monday, July 01, 2019, 22:07
OMEGA = 1663 C
TGHT = 682A, 11.4V
TBHT = 233A, 3.2V
IGP1= 1.5 e-06 Torr
Set autoramp max on TGHT to 730A
Tuesday, July 02, 2019, 08:15
OMEGA =1700 C
TGHT = 730A, 12.0V
TBHT = 233A, 3.2V
IGP1= 1.1 e-06 Torr
Set autoramp max on TGHT to 750A and increments to 0.4A/min
Tuesday, July 02, 2019, 09:49
Temperature on OMEGA began dropping. Changed OMEGA slope to 1.09 (Elog 371) and temperature reading = 1884 C. Aborted autoramp and lowered TGHT current to 740A.
Tuesday, July 02, 2019, 12:14
Temperature and pressure have dropped at a consistent rate.
IGP1= 9.6 e-07 Torr
OMEGA = 1715 C
Will tap up manually to 750A on TGHT
No appreciable increase in pressure will tap back down to 745A on TGHT
Tuesday, July 02, 2019, 13:11
OMEGA = 1675 C
TGHT = 745A, 12.4V
TBHT = 233A, 3.2V
IGP1 = 1.03 e-06Torr
Will start to ramp- down TGHT @ -2.0A/min
OMEGA = 1354 C
TGHT = 495A, 7.01V
TBHT = 233.2A, 3.2V
IGP1= 2.2 e-07 Torr
Continue ramp-down TGHT @ -2.0A/min
Tuesday, July 02, 2019, 17:14
TGHT = 285.5A, 3.4V
TBHT = 232A, 3.1V
IGP1= 1.4 e-07 Torr
Start TBHT ramp-down at -1.0 A/min
Wednesday, July 03, 2019, 08:37
Turned off TGHT and TBHT
IGP1 = 7.8 e-08 Torr
Wednesday, July 03, 2019, 13:18
Final total weight of Target = 1489.5 g
Removed 18 discs after weighing.
|
Monday, June 17, 2019, 17:09, Marla Cervantes, , 49044-9, LP-SIS, Done, Target container calibration/conditioning
|
Monday, June 17, 2019, 17:04
A LP-SIS target container was wrapped with 3 heat shielding layers,
and an empty graphite insert of 17.4 g was introduce in it.
The system was loaded in the EVAP2 and the chamber is currently being evacuated.
The container will be heated to 2000 C in order to correlate the temperature, current and voltage,
as well as to condition the container.
Tuesday, June 18, 2019, 07:28
The TGHT and TBHT current will be tapped to 40 A manually
Autoramp will be set to TGHT 1A/min to 500 A
and TBHT 0.5A/min to 230 A.
Tuesday, June 18, 2019, 20:51
After 2 hours at ~1800 C the container was cooled,
IGP1 = 1.2e-6 Torr
TGHT = 7.16 V, 447.094 A
TBHT = 4.19 V, 233.43 A
Temperature 1793 C
Auto ramp TGHT = -2 A/min, TBHT = -1A/min |
Monday, June 17, 2019, 17:03, Marla Cervantes, , 43943-2, , Done, Graphite insert test
|
Thursday, June 6, 2019, 16:43
A graphite insert with tantalum wires in its caps was loaded in a tantalum tube.
The system will be heated to 2000 C again (see elog 446)
Currently the chamber is being evacuated.
Friday, June 7, 2019, 16:40
Autoramp was set to 450 A at 1A/min to reach 2000 C
The temperature will be hold at 2000 C for a 4 days.
Tuesday, June 11, 2019, 16:46
Autoramp is set to -2 A/min to 0 A
Wednesday, June 12, 2019, 17:01
The tube present sever crystallization but is not broken and has some resistance against pressure. |
Tuesday, June 04, 2019, 08:41, Darwin Ortiz Rosales, Endcaps, , TARGET BOAT, Done, Sintering TaC coating on endcaps and springs
|
Tuesday, June 04, 2019, 08:36
Each endcap is separated with a disc of graphite foil and rolled into packs of 5 within a foil envelope in a target boat.
There are also 4 coated springs, 2 on each side of the stack of endcaps.
The boat is wrapped with 3-layers of Ta heatshields.
Chamber pumped down overnight.
OMEGA slope = 0.99
IGP1 = 3.5e-7 Torr
Will Tap TGHT up manually to 40 A then autoramp to 400A at 1A/min.
Final desired temperature on OMEGA (tap)= 1800C
Tuesday, June 04, 2019, 11:54
IGP1= 6.1e-06 Torr
TGHT= 40 A
Begin autoramp to 400A at 1A/min
Out-gassing cycles observed. Reduced autoramp to 0.5A/min
Currently TGHT=65A, 0.60 V
Wednesday, June 05, 2019, 08:27
TGHT = 321A, 4.9V @1149C
IGP1= 8.49 e-6 Torr
Set autoramp to 1A/min to530 A
Wednesday, June 05, 2019, 13:26
TGHT 530A, 9.2V
IGP1= 3.01e-05 Torr
OMEGA Temperature = 1689 Celsius
Set autoramp to 570A at 1A/min
Wednesday, June 05, 2019, 15:51
Tapped manually to 1800 Celsius
TGHT 579A, 10.1V
IGP1= 2.06e-05 Torr
TGHT tapped down to 575A when OMEGA T ~1810 C
Thursday, June 06, 2019, 08:13
TGHT = 575A, 9.95V
OMEGA = 1809 C
IGP1 = 4.1e-7 Torr
Initiating auto-cool at -2.0A/min
Thursday, June 06, 2019, 16:00
After 1 hour of TGHT at 0A and 0V, unloaded the Target boat.
|
Friday, May 24, 2019, 15:29, Marla Cervantes, , 43943-2, , Done, Graphite insert test
|
Friday, May 24, 2019, 15:26
A graphite insert with tantalum wires in its caps
was loaded in a tantalum tube, the system will be heated to 2000 C
and after 6 hrs at that temperature, it will be cooled and heated to 2000 C again.
The temperature will be hold at 2000 C for a 6 days.
Currently the chamber is being evacuated.
Saturday, May 25, 2019, 06:01
IGP1 = 2.2e-7 Torr
Manually tapping to 50 A
Autoramp set to 1 A/min to 400 A
Saturday, May 25, 2019, 13:37
The autoramp was set to 450 A
Then it was manually tappe to 475 A |
Tuesday, May 21, 2019, 18:01, Marla Cervantes, , 43943-1, , Done, Graphite foil test
|
Tuesday, May 21, 2019, 17:57
A tantalum tube previously coated with TaC and sintered was loaded with graphite foils.
The mass of the foils was 20.04 g.
The system will be heated to 2000 C to find out the corresponding current.
After that the tantalum tube will be trasferred to the EVAP1
and it will be heated there for 5 days.
EVAP2 currently pumping down
Thursday, May 23, 2019, 05:48
IGP1 = 2.516e-7 Torr
Manually tap to 50 A
Autoramp set to 1 A/min to 400 A
Thursday, May 23, 2019, 13:09
IGP1 = 3.78e-6 Torr
TGHT = 6.4 V, 401.3 A
Temperature reading = 1629
Thursday, May 23, 2019, 13:09
Autoramp was set to 550 A at 1 A/min
Stopped at 530 A
Thursday, May 23, 2019, 21:27
IGP1 = 6.77e-7 Torr
TGHT = 9.2175 V, 507.375 A
After 6 hours at ~2000 C the autoramp was set to -2 A/min to 0 A
Friday, May 24, 2019, 8:46
EVAP2 was vented with air and the tantalum tube was removed, examined and transferred to EVAP1 |
Tuesday, May 21, 2019, 14:34, Aaron Schmidt, , , , , HS swap to EVAP 2 flex line.
|
Tuesday, May 21, 2019, 14:33: Install flexible line evap 2 HS. |
Tuesday, May 14, 2019, 13:57, Aaron Schmidt, , , LP-FEBIAD, Done, Test FEBIAD
|
Tuesday, May 14, 2019, 13:56: Removed old HS w/ flexible lines & swapped in the FEBIAD. (HS waterlines are still purged.) Roughing.
Tuesday, May 14, 2019, 14:06: Turbo pump on.
Tuesday, May 14, 2019, 14:22: Waterlines opened. Vacuum ok @ 5.34e-05T & dropping.
Wednesday, May 15, 2019, 06:21
IGP1 = 5.99e-7 Torr,
manually tapping to 40 A.
Autoramp set to 2A/min to TGHT=580 A and TBHT=290 A
Tuesday, May 21, 2019, 08:13
IGP1= 1.43e-7 Torr
TGHT = 580.875 A, 11.22 V
TBHT = 4.45 V, 309.219 A
Temperature 1004 C measured at Ta foil
Ramp-down was initiated with IGP1 = 1.423e-07 Torr
Ramp rate = 2A/min for TGHT and 1/min for TBHT
EVAP2 was vented with air
Tuesday, May 21, 2019, 14:20 Test FEBIAD removed - AS. |
Friday, May 10, 2019, 16:58, Marla Cervantes, , 43943-1, , Done, TaC coating/sintering for graphite insert test
|
Friday, May 10, 2019, 16:54
A tantalum tube was coated with TaC,and wrapped with three tantalum sheets,
the tube was set in the EVAP2 to sinter the TaC coating.
EVAP2 is currently pumping down.
Sunday, May 12, 2019, 18:40
IGP1 = 3.01e-7 Torr
Manually tapped current TGHT to 40 A
IGP1 = 4.89e-Torr
at the IGP1 = 1.961e-6 Torr the autoramp was set to 1 A/min to 380 A
IGP1 = 6.91e-7 Torr
TGHT = 6.133 V, 386.8 A, temperature 1682 C
IGP1 = 7.77e-7
TGHT=6.36V, 399A 1730 C
After 4 hours at 1895 C TGHT = 7.435 V and 445.781 A
TGHT was set -2 A/min to 0 A
The EVAP2 was vented with air and the tube was removed |
Tuesday, April 30, 2019, 09:35, Darwin Ortiz Rosales, Empty, 43044-6, LP-SIS, Done, TaC coating/sintering
|
Tuesday, April 30, 2019, 09:33
Container was coated with TaC and wrapped with 2 Ta heat shields.
Desired temp = 1900 C, Omega slope set = 0.990, Auto ramping TGHT at 1A/min to reach 400A, TGHT will be tapped up accordingly to reach desired Temp.
TBHT will be set fixed at 230A (max). TBHT at 1A/min to reach 230A.
Good vac at 3.0e-5 Torr
Bad vac at 5.0e-5 Torr.
Chamber is currently being pumped down (since yesterday evening).
Tuesday, April 30, 2019, 10:25
Current pressure at IGP1 = 5.17e-7 Torr
Manual tapping to 40A on TBHT and TGHT
TBHT 38.59A, 0.43V
TGHT43.69, 0.23V
waiting for pressure to stabilize.
Tuesday, April 30, 2019, 15:15
Current pressure IGP1= 5.29e-07 Torr
Auto ramping TGHT at 1A/min to reach 400A, and TBHT at 1A/min to reach 230A.
Wednesday, May 01, 2019, 08:41
Target current of 400A reached around 00:19 am
Will tap up to 444A on TGHT as projected from plot of temperature vs current (attachment 1)
Current IGP1=5.91e-07 Torr
Wednesday, May 01, 2019, 09:54
At 444A 1900C not reached. Continue tapping to 1900C (attachment 2)
1900 C reached at 459 A on THGT.
will leave at 1900C for 4 hours.
Wednesday, May 01, 2019, 14:21
IGP1= 6.7e-7 Torr
After 4.5 hours, TGHT was ramped down @ 2A/min and TBHT @1A/min overnight
Thursday, May 02, 2019, 10:46
Vented Evap 2 and removed the target container. |
Tuesday, April 23, 2019, 13:55, Aaron Schmidt, Ta, 43044-4, LP-SIS, In progress, Conditioning Ta#58
|
Ta#58 LP-SIS target description:
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.025mm
Target density = 14.16 g/cm3
Target length = 3.4 cm
Total Mass = 48.138 g [Incl foils + Ta wire on 6 packs]
Total mass w/ Target oven= 464 g
Discs in target are arranged as follows: 1pack / 75singles / 1pack / 100singles / 2packs / 100singles / 1pack / 75singles / 1pack
End caps installed (not yet expanded). No Ta heat shield added.
Tuesday, April 23, 2019, 13:54: Roughing.
Tuesday, April 23, 2019, 14:01: Turbo pump started.
Tuesday, April 23, 2019, 14:09: Turbo pump at speed.
TBHT will be ramped up to 230A at 1.0A/min.
TGHT will be ramped up to 650A at 2.0A/min.
Final desired temperature = 1900C.
OMEGA slope = 0.98.
Wednesday, April 24, 2019, 08:38: Power / sources on.
Wednesday, April 24, 2019, 08:43: TGHT manually to 40A. Vacuum @ 1.87e-07T.
Wednesday, April 24, 2019, 08:45: Auto-ramping TGHT / TBHT @ 2 / 1 A per min to 350 / 180 A.
Slope found / set. Slope = 0.98. Laser on target, OK.
Wednesday, April 24, 2019, 11:58: Vacuum @ 4.45e-07T. Temp @ 1120 deg C. TGHT / TBHT @ 350 / 180 A.
Wednesday, April 24, 2019, 12:02: Auto-ramping TGHT / TBHT @ 2 / 1 A per min to 650 / 230 A.
Wednesday, April 24, 2019, 14:27: Halted auto ramping briefly. Set auto-ramping TGHT @ 2 A per min to 630 A .
Wednesday, April 24, 2019, 14:32: TGHT / TBHT @ 630 (627.9) / 230 (233.3) A.
Vacuum @ 1.15e-06T. Temp @ 1840 deg C. Hold.
Thursday, April 25, 2019, 06:59: Vacuum @ 2.74e-07T. Temp @ 1860 deg C. Hold.
Thursday, April 25, 2019, 08:05: Auto-ramping TGHT @ 2 A per min to 640 A.
Thursday, April 25, 2019, 08:13: TGHT / TBHT @ 640 (636.9) / 230 (233.16) A.
Vacuum @ 9.96e-07T. Temp @ 1878 deg C.
Thursday, April 25, 2019, 08:15: Auto-ramping TGHT @ 2 A per min to 645 A.
Thursday, April 25, 2019, 08:20: Auto-ramping TGHT @ 2 A per min to 650 A.
Thursday, April 25, 2019, 08:24: Vacuum @ 9.96e-07T. TGHT / TBHT 653 (650.3) / 230 (233.16) A. TGHT Voltage= 12.760V. Omega: 1902-1903 deg C. Desired temperature = 1900C reached.
Thursday, April 25, 2019, 14:00: Begin auto-cooling TGHT / TBHT @ -2 / -1 A per min.
Friday, April 26, 2019, 10:29: Power/heaters off. Turbo pumps off.
Friday, April 26, 2019, 10:42: Venting. |
Wednesday, April 17, 2019, 09:06, Marla Cervantes, , 38295-10, LP-FEBIAD, Done, Graphite insert test
|
Wednesday, April 17, 2019, 09:03
An uncoated target container was loaded with a graphite insert and wrapped with 3 tantalum layers,
Two Ta caps were used
EVAP2 was pumped down, IGP1 = 5.14e-7 Torr
The TGHT and TBHT current was tapped to 40 A manually
Autoramp was set to TGHT 1A/min to 500 A
and TBHT 0.5A/min to 230 A.
The temperature reached 2000 C as planned
the target container stayed at that temperature for 1 week.
Tuesday, April 23, 2019, 10:00
EVAP2 was vented and the target container was removed.
The container crystalized but did not break. |
Tuesday, April 16, 2019, 13:40, Aaron Schmidt, , , , , Replace bottom insert on HS
|
Tuesday, April 16, 2019, 13:38: Replaced the bottom insert on the heat shield.
Used small amount of isopropyl alcohol to wipe the inside if the HS out. |
Sunday, April 07, 2019, 08:13, Marla Cervantes, , 43630-5, , Done, Graphite insert test #5
|
Sunday, April 07, 2019, 08:10
A graphite insert (with conical caps) was loaded in tantalum tube previously coated with TaC,
and wrapped with 3 tantalum foils,
a tanalum cap was inserted in one side of the Ta tube and sealed.
The tube was set in the EVAP2 and the furnace was pumped down.
IGP1 = 1.24e-7 Torr.
The current was tapped to 40 A
Autoramp was set to 1 A/min to 300 A.
At TGHT 335.53 S, 5.28 V the temperature was 1560
The autoramp was set to 450 A.
At TGHT 474.75 S, 7.96 V the temperature was 1560
The autoramp was set to 450 A.
To reach 2000 C, TGHT = 500.25 A, 8.45 V.
After 1hr the temperature stabilized to 1959 C
and the current was increased to TGHT = 510.28 A, 8.64 V.
After stabilization the temperature reached 2010 C.
The current was decreased to TGHT = 503.15 A, 8.45 V
and the temperature stabilized to 2001 C.
The voltage increased unexpectedly to 8.89 V and the temperature increased to 2055,
the current was reduced to keep the tube at 2000 C.
The voltage kept increasing and we kept decreasing the current to keep the tube at 2000
The final current before venting and getting out the container was
TGHT = 466.219 A and 8.467 V.
Test result: Broken tantalum tube. |
Wednesday, April 03, 2019, 16:59, Marla Cervantes, TaC, 43630-5, , Done, TaC coating/sintering for graphite insert test
|
Wednesday, April 03, 2019, 16:57
Tantalum tube was coated with TaC and wrapped with Ta heat-shield (3 layers)
Desired temp = 1900 C (expected TGHT ~445A/7.5V).
EVAP2 currently pumping down.
Thursday, April 04, 2019, 05:12
IGP1 = 4.5e-7 Torr
The current is tapped manually to 40 A
After1 hour IGP1 = 1.18e-6 Torr, the autoramp was set to 1 A/min to 400 A
Thursday, April 04, 2019, 18:58
After 4 hours at ~1900 C:
IGP1 = 6.13e-7 Torr
TGHT = 6.74 V, 416.06 A |
Monday, April 01, 2019, 16:35, Darwin Ortiz Rosales, , 43630-4, , Done, TaC coating/graphite/sintering
|
Monday, April 01, 2019, 16:35
Container was coated with TaC and a roll of graphite inserted inside the tube. A couple of TaC coated Ta springs inside to keep graphite pressed against walls of cylinder.
Container wrapped with 2 Ta heat shields.
Desired temp = 1900 C, Omega slope set = 0.990, Auto ramping TGHT at 1A/min to reach 400A, TGHT will be tapped up accordingly to reach desired Temp.
Good vac at 3.00-5 Torr
Bad vac at 5.0e-5 Torr.
Chamber is currently being pumped down. Sintering will proceed tomorrow.
Tuesday, April 02, 2019, 06:27
IGP1 = 4.37e-7 Torr
Current is manually tapped to 40 A
Tuesday, April 02, 2019, 08:12
Pressure increased to IGP1 = 1.15e-5 Torr
and it stabilized to IGP1 = 2.32e-6 Torr after ~1.5 hrs
Autoramp is set to 1 A/min to 400 A
Tuesday, April 02, 2019, 08:45
Autoramp stopped momentarily, to stop current reduction
When pressure reduced to ~4e-5Torr, current was tapped manually to 50 A
Autoramp is set again, the conditions are
IGP1 = 2.5e-5 Torr
TGHT = 58.87 A, 0.36 V
Tuesday, April 02, 2019, 09:31
Autoramp stopped momentarily, to avoid current reduction
When pressure reduced, autoramp is set again,
the conditions are:
IGP1 = 2.9e-5 Torr, TGHT = 0.52 V, 71.5 A
Tuesday, April 02, 2019, 15:32
Autoramp stopped momentarily, to avoid current reduction
conditions: IGP1=4.99e-5 Torr, TGHT = 0.78 V, 85.9 A
When pressure reduced, autoramp is set again,
Tuesday, April 02, 2019, 22:37
Camera conexion was lost
Autoramp reached 400 A
the current was manually raise to 425 A to allow the completation of the process
Wednesday, April 03, 2019, 00:27
Camera connection still off
The current was reduced to 410 A to match with the estimated temperature
Wednesday, April 03, 2019, 06:56
Camera connection is back, temperature reading is 1786 C
IGP1 5.01e- Torr
TGHT = 6.93 V, 412.22 A
Autoramp was set to -1A/min to 0A
Wednesday, April 03, 2019, 11:01
IGP1 = 1.67e-7 Torr
TGHT = 2.25 V, 179.53 A
Autoramp changed to -2 A/min
Wednesday, April 03, 2019, 16:54
The tube was removed from the EVAP2,
The coating has a different color than regular coatings, but it doe not seem like the graphite adhered as expected. |
Monday, March 18, 2019, 15:58, Darwin Ortiz Rosales, ZrC, 43044-5, LP-SIS, Done, Sintering ZrC
|
Monday, March 18, 2019, 15:51
Total number of foils: 555
Total mass of material including graphite foils: 478 grams
Total length packed 14.2 cm
container has 3 Ta heat shields.
No endcaps inserted to facilitate outgassing
Two TaC coated Ta wire springs inserted at either end to allow for ZrC expansion.
5 extra foils tucked beneath each spring for QC; total mass (10 discs) =1.0160 g
Desired temp = 1900 C, Auto ramping TGHT at 0.1 A/min to reach 280A A (Omega slope set = 0.990, approx 1400 C, Elog#427), TGHT will be tapped up accordingly to reach desired temperature.
TBHT will be set fixed at 230A (max). TBHT at 0.1 A/min to reach 230A.
Good vac at 3.00-5 Torr
Bad vac at 5.0e-5 Torr.
Currently being pumped down.
Tuesday, March 19, 2019, 08:57
Current pressure IGP1 = 5.24e-07 Torr
Manually tapping to 40A on TBHT and TGHT
At 20 A IGP1 pressure trending up. Will leave at 20A until trending down.
Pressure @ 20 A set, peaked ~1.8e-06 Torr after 1 hour
Tuesday, March 19, 2019, 10:32
Tapping manually to 50 A on TBHT and TGHT while monitoring IGP1 pressure
Tapped to 25 A and IGP1 pressure trending up. Will allow to stabilize.
Tuesday, March 19, 2019, 11:34
Pressure stabilized at ~3.25e-06 Torr
Tapped up to 30 A on both TGHT and TBHT
Pressure stabilized at ~6.6e-06
Tapped up to 34A on both TGHT and TBHT
Pressure stabilized at ~1.2e-05 Will allow to drop before proceeding
Tuesday, March 19, 2019, 13:43
Tapped up to 40A waiting for pressure to stabilize
Pressure shot up ~8.5e-05, therefore tapped down TGHT to 35A (At 35A TGHT current value fluctuates, probably better to ramp up to 36A)
Will let pressure drop before proceeding with TGHT heating
Ramped TGHT to 36A, IGP1 pressure still trending down and current measurements stable.
Starting autoramp at 0.3A/min for both TGHT and TBHT until 280A and 230A respectively
Initial TGHT Current: 33.6A, 0.05V
Initial TBHT Current: 38.6A, 0.48V
IGP1 = 4.9e-05 Torr
Wednesday, March 20, 2019, 09:41
TGHT has only ramped to 45.7 A, 0.085V
TBHT has only ramped to 50.2A, 0.62V
IGPI pressure ~4.0 e-5 Torr
Stopping ramp and monitoring pressure to see if it drops appropriate levels.
Wednesday, March 20, 2019, 14:10
IGP1 pressure = 7.6e-06 Torr
TGHT 47.7Z, 0.16V
TBHT 50.1A, 0.63V
Autoramp at 0.1A/min both TGHT and TBHT to 280A and 230A respectively.
Thursday, March 21, 2019, 08:12
IGP1 = 3.1e-05 Torr
TGHT = 51.4 A, 0.18V
TBHT=61.9A, 0.87V
Stopped autoramp
Manually ramping TGHT and TBHT while monitoring pressure
Rampted up TGHT to 54A (reading 65 A), 0.5V and TBHT to 68A, 0.9V
Allowing pressure to stabilize
Manually tapped TGHT to 80A, .81V
Manually tapped TBHT to 90A, 1.3V
IGP1 = .0002 Torr
Will leave over night to allow pressure to drop
Friday, March 22, 2019, 08:17
IGP1 = 6.6e-06
TGHT = 88.8A, 0.81V
TBHT = 90.1A, 1.3V
Will manually tap ~100A on both TBHT and TGHT
Friday, March 22, 2019, 12:18
IGP1 = 1.28e-05 Torr
TGHT = 100.9A, 1.0V
TBHT = 101.2A, 1.5V
will allow pressure to drop slightly the autoramp at 0.1A/min for both TGHT and TBHT until 280A and 230A respectively
Friday, March 22, 2019, 14:51
IGP1= 7.4 e-06 Torr
TGHT = 100.8A, 1.0V
TBHT= 101.5A, 1.5V
Started autoramp at 0.1A/min for both TGHT and TBHT until 280A and 230A respectively
Tuesday, March 26, 2019, 08:18
IGP1 oscillated around ramping trip point 3.0e-05 while current slowly ramped to 280A (reached sometime during the night).
IGP1= 7.8e-06 Torr
TGHT= 283.4A, 4.2V
TBHT= 233.1A, 4.1V
Will continue ramp TGHT @0.2A/min up to 400A (Omega slope set = 0.990, approx 1800 C, Elog#427)
Wednesday, March 27, 2019, 09:39
Target has been at 400A, OMEGA ~1400C since ~7pm of previous evening
TGHT = 400.2A, 6.45V
TBHT= 233.1A, 4.16V
IGP1= 3.1e-07 Torr
Autoramp TGHT to440A @0.2A/min
Stopped autoramp at TGHT = 427.4 A and 7.00V, OMEGA= 1492 C
Wednesday, March 27, 2019, 14:14
Restarted TGHT autoramp @.2A/min up to 440A
Friday, March 29, 2019, 12:06
Changed OMEGA slope to 1.09 after checking with the analog pyrometer
IGP1 = 1.65e-07 Torr
TGHT = 441.3A, 7.5V
TBHT= 233.0A, 4.2V
Tapping TGHT to 450A @ ~1A/min while monitoring pressure
TGHT remained at 451A, 7.8 V and TBHT at 233.2A, 4.2 V, for 10.5 hours while OMEGA Temperature ~1810 C.
Ramp-down was initiated with IGP1 = 1.7e-07 Torr
Ramp rate = 2A/min for TGHT and 1/min for TBHT
Monday, April 01, 2019, 08:53
TGHT = 0A, 0.05V
TBHT= 0.01A, 0V
IGP1= 4.05e-08 Torr
Unloading Target
Target Final weight = 473 g
% Mass of ZrC+C+organics lost = 14.20 % compared to 13.95% theoretical organics content.
Final weight of 10 discs = 0.9250 g
% mass lost on this discs = 13.66%
The tube was slightly bent along the short axis
The discs expanded but more towards one side (possibly due to discrepancy in spring strength).
One protective graphite disc added to each end
One end cap on each end |
Wednesday, March 13, 2019, 15:43, Marla Cervantes, , 43630-6, , Done, Graphite insert test #4
|
Wednesday, March 13, 2019, 15:41
An uncoated tantalum tube was loaded with a graphite insert (with conical caps).
3 tantalum foils were wrapped around the tantalum tube and a Ta cap was added.
EVAP2 is currently pumping down
The tube will be hated for 5 days at 2000 C
Thursday, March 14, 2019, 10:07
IGP1 = 5.37e-7 Torr
The TGHT will be tapped manually to 50 A
After aprox 1 hour IGP1 = 5.08e-7 Torr, TGHT=46.5 A, 0.224 V
Autoramp is set to 1A/min to 300 A
Autoramp is set to 1A/min to 450 A
Autoramp was stopped at 425 A when 2000 C were achieved
Sunday, March 17, 2019, 00:25
IGP1 = 2.03e-7 Torr
TGHT=424.2 A, 7.117 V, temp 1976 C
Sunday, March 17, 2019, 15:04
IGP1 = 21.6e-7 Torr
TGHT=424.1 A, 7.085 V, temp 1967 C
cooling down -1 A/min |
Thursday, March 07, 2019, 09:22, Darwin Ortiz Rosales, Empty, 40282-4, TARGET BOAT, Done, Transfer tube TaC coating (Legnaro)
|
Thursday, March 07, 2019, 09:09
Transfer tube from Legnaro was coated with TaC.
The transfer tube was set in a tantalum boat and wrapped with 3 heat shields,
the legs of the transfer tube were let out of the shielding sheets.
Chamber pump down was started on Wednesday March 06, 2019.
Desired temperature TGHT = 1800 C, Omega slope set = 0.990.
IGP1= 4.48e-07 Torr
Will tap up TGHT manually to 40-50 A and monitor pressure.
Thursday, March 07, 2019, 10:57
The TGHT current was left at 40 A for 50 min, the pressure achieved was 6.15e-7 Torr
The TGHT was rised to 45 A 11:00 am the pressure rised to 6.18e-7 Torr (11:10am)
The TGHT was rised to 50 A 11:10 am the pressure rised to 6.81e-7 Torr (11:32am)
auto ramp was set to 1 A/min to 300 A
Good vacuum 3e-5 Torr
Bad vaccum 5e-5 Torr
auto ramp was set to 1 A/min to 400 A
auto ramp was set to 1 A/min to 470 A
Final conditions TGHT = 485 A, 8.25V Temperature = 1800 C
The transfer tube stayed at 1800 C for 4 hours
auto ramp was set to -1 A/min to 0 A.
Friday, March 08, 2019, 16:53
EVAP2 was vented with air and the transfer tube was unloaded |
Thursday, February 21, 2019, 09:15, Darwin Ortiz Rosales, Empty, 42464-4, HP-FEBIAD, Done,
|
Thursday, February 21, 2019, 09:01
Container coated with TaC and wrapped with 2 Ta heat shields.
Desired temperature= 1900 C, Omega Slope set = 0.990, Auto TGHT at 0.2A/min to reach 400A, TGHT will be tapped up accordingly to reach desired Temp.
TBHT will be set fixed at 230 A (max).
Good vac at 3.00e -5 Torr
Bad vac at 5.00e-5 Torr
Chamber pump down was started on Wednesday February 20th; however, this morning IEVAP2:TP1 and IEVAP2:BV1 were found in the OFF position.
There are no abnormal sounds from the roughing pump.
IGP1= 5.6e-2 Torr
Will turn on IEVAP2:BV1 and IEVAP:TP1 from the hot lab and listen for anything out of the ordinary.
Friday, February 22, 2019, 09:56
Pumped down to IGP1=2.1 e-07
Will tap up TGHT and TBHTmanually and monitor the pressure.
Friday, February 22, 2019, 11:20
Manually tapped up TGHT (V~ 0.90) and TBHT(V ~0.99) to 90A
maximum pressure reached ~7.4e-06 Torr and trended down
Friday, February 22, 2019, 11:25
Initiating Autoramp @ 0.2 A/min for TGHT to reach 450A and TBHT to reach 230A
Estimated temperature for TGHT ~1200 C
Friday, February 22, 2019, 15:42
TGHT @ 145 A and TBHT @ 138A
Changed Autoramp to 0.1 A/min so that it will take over the weekend to reach 450A and 230A for TGHT and TBHT respectively.
Monday, February 25, 2019, 08:29
IGP1=1.1e-07 Torr, TGHT= 451.4 A, 6.7 V, TBHT = 233.1 A, 3.1 V
Omega T = 1197 C
Will manually tap up by increasing TGHT current by ~1A/min monitoring pressure. Will allow system to stabilize ~1400 C.
Monday, February 25, 2019, 11:14
Trend forcast 1400 C at TGHT= 566.75 A (Line plot attached)
Actual but not stable ~1445-1452 C at 566 A
Will continue to manually increase current monitoring pressure
Monday, February 25, 2019, 12:33
Omega T= 1679 C , TGHT = 657.7A, 10.52 V, TBHT = 233.2 A, 3.2 V
IGP1 = 1.4e-05 Torr slightly trending up.
Autoramp @ 1 A/min to a maximum of TGHT 780 A.
Monday, February 25, 2019, 14:43
IGP1= 3.7e-06 Torr trending down slightly, TGHT = 780.3 A, 12.9 V
Omega T = 1931 C
Monday, February 25, 2019, 15:14
manually tap up to TGHT to 790 A
Monday, February 25, 2019, 15:36
IGP1= 2.9e-6 Torr trending down
TGHT = 784.3 A, 13.01 V
TGHT current set to 790 A
Omega T = 1940 C
Will leave over-night
Tuesday, February 26, 2019, 08:23
IGP1= 7.85e-07 Torr Stable
TGHT = 784.32 A, 12.54 V
TBHT = 233.3 A, 3.2 V
OMEGA T = 1948 C
Initiating Auto-cool ramp at 2.0A/min and 1.0A/min for TGHT and TBHT respectively.
Wednesday, February 27, 2019, 08:10
IGP1 = 3.3 e-08 Torr Stable
TGHT = 0A, 0.05V
TBHT = 0.02A, 0. V
Will begin vacuum release
|
Wednesday, February 13, 2019, 10:08, Darwin Ortiz Rosales, , 43630-1 , , Done, Graphite insert test 3b
|
Wednesday, February 13, 2019, 10:04
A previously coated tantalum tube with 3 layers of shielding (Details in e-log 426) was loaded with a graphite insert.
The tube was loaded in evaporator 2 and pumped down
The graphite insert will be heated to 2000 C for 1 week
IGP1=1.37e-07 Torr
Wednesday, February 13, 2019, 10:27
IGP1= 1.46e-07 Torr
Manual tapping to 40A on TGHT
TGHT 40.7A, 0.104V
Autoramp started at 1A/min up to 400 A
Good Vacuum = 3.00e-05, Bad Vacuum = 5.00e-05
Thursday, February 14, 2019, 08:42
IGP1= 2.2e-07 Torr, T=1705 C, TGHT 401A, 6.7 V
Manually tapping to 2000 C (Slow ~1 A/min) in 5 A increments followed by waiting for equillibrium
Thursday, February 14, 2019, 10:54
IGP1 = 1.4e-06 Torr, T = 2003 C, TGHT 500A, 9.1 V
Waiting for equillibrium
manually tapped TGHT to 503A, T = 2003 C
Will leave for 1 week
Wednesday, February 20, 2019, 08:44
IGP1= 1.37e-07 Torr, T=1943 C, THGT= 503 A, 8.9 V
Ramp-down @ 2A/min
Wednesday, February 20, 2019, 14:02
1 hour since TGHT = 0 A
Venting will proceed.
|
Thursday, February 07, 2019, 15:20, Darwin Ortiz Rosales, Empty, 43630-1, , Done, TaC coating/sintering
|
Thursday, February 07, 2019, 14:12
Tantalum tube coated with TaC and wrapped with 3 layers of Ta heat-shielding.
Desired temperature= 1900 Celsius (expected TGHT ~445A/7.5V)
EVAP2 Currently pumped down, heating will be initiated tomorrow.
Friday, February 08, 2019, 08:46
Current pressure IGP1 = 3.46e-07 Torr
Manual tapping to 50A on TGHT
TGHT 47.43A, 0.26V
Waiting for pressure to stabilize.
Pressure was going down so current was increased manually to 65 A to induce the outgassing.
TGHT 73.9A, 0.67V
MAx pressure IGP1 = 4.41e-6 Torr
After approx 1 hour
TGHT = 0.70 V 74.1 A
IGP1 = 1.63 e-6 Torr
Autoramp was set to 2 A/min for final current of 350 A
Friday, February 08, 2019, 13:43
Autoramp TGHT reached 350 A /5.47 V, current temperature at 1660 Celsius
IGP1 = 3.0e-06 Torr/coming down
Increase TGHT to 400 A autoramp at 2A/min
Friday, February 08, 2019, 14:39
TGHT reached 413 A, 6.8 V, pressure at 1.9 e-06 Torr coming down
Continue to tap up TGHT to reach 1900 C
Friday, February 08, 2019, 14:56
TGHT manually increased to 428 A, 7.18V, pressure at 2.0e-06 Torr coming down slowly
Temperature at 1903 C
Will continue to heat at ~1900 C for four hours before cooling down
Friday, February 08, 2019, 21:00
TGHT 7.21 V, 429.75 A, 1873 C
IGP1 6.77e-7 Torr
The heater ramp is set to -2 A/min to 0 A. |
Wednesday, January 23, 2019, 13:06, Marla Cervantes, , 43630-2, , Done, Graphite insert test #3
|
Wednesday, January 23, 2019, 13:01
A previously coated tantalum tube with 3 layers of shielding (Details in e-log 426) was loaded with a graphite insert.
The tube was loaded in evaporator 2 and pumped down
The graphite insert will be heated to 2000 C for 3 weeks
Thursday, January 24, 2019, 10:04
Pressure = 3.66e-7 Torr
TGHT manually tapped to 45 A
Final pressure = 3.8e-7 Torr
Set autoramp to 350 A @ 2A/min
TGHT = 1643 C
Set autoramp to 400 A @ 2A/min
TGHT = 1790 C
Started to tapped manually at approx 5 A every 30 s
Final TGHT => 1896 C, 8.16 V, 480.46 A
The current will stay at 480 A until temperature stabilizes.
The current was reduced to 476 A to stay at 1900 C
Friday, January 25, 2019, 17:16
Pressure = 3.22e-7 Torr
TGHT = 8.17 V, 477.65 A, 1882 C
Monday, January 28, 2019, 09:09
Pressure = 1.67e-7 Torr
TGHT = 8.07 V, 477.65 A, 1859 C
The temperature readings are fluctuating between 1880 and 1859 C
Tuesday, January 29, 2019, 07:32
Pressure = 1.55e-7 Torr
TGHT = 8.17 V, 477.75 A, 1880 C
Tuesday, January 29, 2019, 11:34
Pressure = 1.55e-7 Torr
TGHT = 8.27 V, 477.56 A, 1897C
Tuesday, January 29, 2019, 12:47
Pressure = 1.53e-7 Torr
TGHT = 8.19 V, 477.75 A, 1899C
Tuesday, January 29, 2019, 13:38
Pressure = 1.55e-7 Torr
TGHT = 8.25 V, 477.75 A, 1905C
Thursday, January 31, 2019, 16:12
Pressure = 1.40e-7 Torr
TGHT = 8.4 V, 476.81 A, 1918C
Thursday, January 31, 2019, 22:32
Pressure = 1.39e-7 Torr
TGHT = 8.37 V, 476.71 A, 1914C
The current will be ramped down @1 A/min
Friday, February 01, 2019, 09:58
Last 22 A tapped to 0 manually
Tantalum tube was removed from the EVAP2 |
Friday, January 18, 2019, 15:11, Darwin Ortiz Rosales, Empty, 43044-5, LP-SIS, Done, TaC coating/sintering (training/online use)
|
Friday, January 18, 2019, 15:00
Container was coated with TaC and wrapped with 3 Ta heat shields.
Desired temp = 1900 C, Omega slope set = 0.990, Auto ramping TGHT at 1A/min to reach 400A, TGHT will be tapped up accordingly to reach desired Temp.
TBHT will be set fixed at 230A (max). TBHT at 1A/min to reach 230A.
Good vac at 3.00-5 Torr
Bad vac at 5.0e-5 Torr.
Chamber is currently being pumped down. Sintering will proceed next week.
Monday, January 21, 2019, 10:17
Current pressure at IGP1 = 1.31e-7 Torr
Manual tapping to 50A on TBHT and TGHT
TBHT 38.75A, 0.41V
TGHT 37.5A, 0.07V
waiting for pressure to stabilize.
pressure IGP1 8.0 e-7 Torr
Auto ramping TGHT at 1A/min to reach 400A, and TBHT at 1A/min to reach 230A.
Tuesday, January 22, 2019, 09:34
TGHT reached 400A , 1800 C, however temperature dropped to 1785 C.
TGHT increased to 444A manually. Temperature stabilized at 1880 C.
After 10 hours, TGHT was ramped down @ 2A/min and TBHT @1A/min
Tuesday, January 22, 2019, 14:36: Evap 2 PS off. Turbo off (Around 14:10) Vented Evap 2 and removed the target container with Darwin. - AS.
|
Wednesday, January 16, 2019, 11:53, Marla Cervantes, TaC, 43630-2, , Done, TaC coating/sintering for graphite insert test
|
Tuesday, January 15, 2018, 17:30
Tantalum tube was coated with TaC and wrapped with Ta heat-shield (3 layers)
Desired temp = 1900 C (expected TGHT ~445A/7.5V), TBHT will be set fixed at 230A (max).
EVAP2 currently pumping down.
Pressure at IGP1 4.71 -7 Torr.
Tapped up TGHT manually to 40 A
Waited ~1 hr for vacuum to stabilize.
IGP1 = 9.96-7 Torr
Good vac at 3.00e-5 Torr
Bad vac at 5.00e-5 Torr.
Initiating auto ramp for TGHT @ 1 A/min to a max set point of 350 A
Once max set points achieved, will tap up manually to final desired temperature of 1900 C
Thursday, January 17, 2019, 15:31
The tube remained at ~1900 C for 6 hours.
IGP1=5.8e-7 Torr
TGHT = 427 A, 7.23 V
Min Temperature = 1890 C
Thursday, January 17, 2019, 15:33
Auto-ramp set to TGHT 0 A @ -2 A/min. |
Thursday, December 20, 2018, 10:27, Marla Cervantes, , 43630-6, , Done, Tantalum tube heating
|
Thursday, December 20, 2018, 10:24
A tantalum tube was loaded in evaporator 2 on Wednesday 19/Dec/2018.
It is going to be heated to 2000 C during 3 weeks
Pressure IGP1 = 4.88e-7 Torr
TGHT manually tapped to 40 A
Autoramp set to 2 A/min on TGHT to 400 A aiming for 1800 C
The system tripped due to a power outage.
the current went from 57 to 0 A.
The tube did not show damage signs.
This experiment will be postponed. |
Thursday, November 22, 2018, 10:19, Marla Cervantes, , 43630-7 , , Done, Graphite insert test #2
|
Thursday, November 22, 2018, 10:12
A previously sintered tantalum tube with 3 layers of shielding was loaded with a graphite insert.
The tube was loaded in evaporator 2 on Wednesday 21/11/2018 and pumped down
The graphite insert will be heated to 2000 C
current pressure IGP1 = 4.2e-7 Torr
TGHT manually tapped to 40 A
Autoramp set to 2 A/min on TGHT to 400 A aiming for 1800 C
Thursday, November 22, 2018, 17:13
TGHT 401.25 A, 6.79 V
Temperature 1780 C
IGP1 7.89e-7 Torr
Tapping manually to reach 1800 C, final current 407.2 A, 6.96 V
Friday, November 23, 2018, 17:13
Tapped manually to TGHT 469.0 A, 8.64 V
Temperature 2019 C
IGP1 2.68e-7 Torr
Thursday, November 29, 2018, 08:03
TGHT 469.0 A, 8.945 V
Temperature 2061 C
IGP1 2.12e-7 Torr
Tuesday, December 04, 2018, 07:53
TGHT 469.1 A, 8.814 V
Temperature 1983 C
IGP1 1.52e-7 Torr
Wednesday, December 05, 2018, 21:30
TGHT 469.1 A, 8.75 V
Temperature 1983 C
IGP1 1.22e-7 Torr
Thursday, December 06, 2018, 12:25
TGHT 468.9 A, 8.66 V
Temperature 1977 C
IGP1 1.42e-7 Torr
Friday, December 07, 2018, 17:59
TGHT 468.9 A, 8.80 V
Temperature 1977 C
IGP1 1.42e-7 Torr
Wednesday, December 12, 2018, 12:18
TGHT 469.2 A, 8.7 V
Temperature 1945 C
IGP1 1.10e-7 Torr
Thursday, December 13, 2018, 10:42
TGHT 469 A, 8.7 V
Temperature 1939 C
IGP1 1.04e-7 Torr
Ramping temperature down at -2 A/min
Friday, December 14, 2018, 10:42
TGHT 0.0 A, 0.051 V
IGP1 4.36e-8 Torr |
Monday, November 19, 2018, 12:57, Marla Cervantes, Empty, 43630-7, , Done, TaC coating/sintering for graphite insert test
|
Monday, November 19, 2018, 08:57
Tantalum tube was coated with TaC and wrapped with Ta heat-shield (3 layers)
Desired temp = 1900 C (expected TGHT ~445A/7.5V), TBHT will be set fixed at 230A (max).
Pressure at IGP1 2.61-7 Torr.
Tapped up TGHT and TBHT manually to 40 A
Waited ~1 hr for vacuum to stabilize.
IGP1 = 4.27e-7 Torr
Good vac at 3.00e-5 Torr
Bad vac at 5.00e-5 Torr.
Initiating auto ramp for TGHT @ 1 A/min to a max setpoint of 350 A
Once max setpoints achieved, will tap up manually to final desired temperature of 1900 C
Monday, November 19, 2018, 18:14
Temperature was 1755 C at 350 A
IGP1 = 9.28e-7 Torr
Tapped manually to 393 A (6.83 V)
IGP1 = 1.4e-6 Torr
Temperature 1904 C
The tube will stay at max current point overnight.
Tuesday, November 20, 2018, 08:17
IGP1 = 9.28e-7 Torr
TGHT = 395 A, 6.98 V
Temperature 1903 C
Auto-ramp set to TGHT 0 A @ -2 A/min. |
Friday, November 02, 2018, 17:36, Marla Cervantes, Empty, 39530-1, LP-FEBIAD, Done, Graphite insert test #1
|
Friday, November 02, 2018, 17:33
A new LP-FEBIAD was coated and syntered (e-log 421 Evaporator_2)
The container was loaded with an empty graphite insert.
Graphite insert mass = 24.1724 g
A current of 440 A TGHT and 230 A TBHT will be inputed to the container
EVAP2 currently pumping down
Saturday, November 03, 2018, 08:04
IGP1 = 5.66e-7 Torr
Tapping manually to 40 A on TGHT and TBHT
Then auto/ramp wiill be set to 2 A/min on TGHT and 1 A/min on TBHT
Maximum temperature achieve 1802 C
Tuesday, November 06, 2018, 14:49
Container has reduced and increased its temperature from ~1760 to 1802 C.
IGP1 3.44e-7 Torr
TGHT 441.7 A and 7.7 V
TBHT 233.2 A and 3.2 V
Wednesday, November 07, 2018, 08:32
Temperature 1785 C
IGP1 2.90e-7 Torr
TGHT 441.38 A and 7.7 V
TBHT 233.2 A and 3.2 V
Friday, November 09, 2018, 17:26
Temperature 1787 C
IGP1 2.12 -7 Torr
TGHT 442.03 A and 7.7 V
TBHT 233.06 A and 3.19 V
Tuesday, November 13, 2018, 14:13: Turbos, power supplies off. Prepare for venting. |
Wednesday, October 31, 2018, 19:35, Marla Cervantes, TaC, 39530-1, LP-FEBIAD, Done, TaC coating/sintering for graphite insert test
|
Wednesday, October 31, 2018, 19:35
Container is coated with TaC and wrapped with Ta heat-shield (3 layers)
Desired temp = 1900 C (expected TGHT ~445A/7.5V), TBHT will be set fixed at 230A (max).
Chamber is currently being pumped down
Thursday, November 01, 2018, 10:31
Pressure at IGP1 9.44e-7 Torr.
Tapped up TGHT and TBHT manually to 40 A
Thursday, November 01, 2018, 12:32
Waited ~1 hr for vacuum to stabilize.
IGP1 = 1.42e-6 Torr
Good vac at 3.00-5 Torr
Bad vac at 5.0e-5 Torr.
Initiating auto ramp for TGHT @ 1 A/min to a max setpoint of 350 A
Initiating auto ramp for TBHT @ 0.5 A/min to a max setpoint of 230 A
Once max setpoints achieved, will tap up manually to final desired temperature of 1900 C
Tapped manually to 445 A, Temperature 1896 C.
Friday, November 02, 2018, 07:35
TGHT 7.86 V 445.6 A
TBHT 3.22 V 233.3 A
IGP1 1e-6 Torr
Ramping down TGHT and TBHT to 0 A @ 2 A/min.
Friday, November 02, 2018, 17:28
Monday, October 29, 2018, 12:39
Venting EVAP2, TaC coat sintering completed. |
Thursday, October 25, 2018, 15:37, Marla Cervantes, TaC, 43044-7, LP-SIS, Done, TaC coating/sintering for graphite insert test
|
Thursday, October 25, 2018, 10:36
Container is coated with TaC and wrapped with Ta heat-shield (3 layers)
Desired temp = 1900 C (expected TGHT ~445A/7.5V), TBHT will be set fixed at 230A (max).
Chamber is currently being pumped down
Friday, October 26, 2018, 08:40
Pressure at IGP1 1.06e-6 Torr.
Tapped up TGHT and TBHT manually to 40 A
Waited 1 hr for vacuum to stabilize.
IGP1 = 8.9e-6 Torr
Good vac at 3.00-5 Torr
Bad vac at 5.0e-5 Torr.
Initiating auto ramp for TGHT @ 1 A/min to a max setpoint of 350 A
Initiating auto ramp for TBHT @ 0.5 A/min to a max setpoint of 230 A
Once max setpoints achieved, will tap up manually to final desired temperature of 1900 C
Friday, October 26, 2018, 10:46
At 62 A, the vacuum overpassed the "Bad vacuum " limit and the current reduced to 54 A.
when the pressure returned to the "Good vac" limit the ramping started automatically.
Friday, October 26, 2018, 16:59
TGHT= 450 A, Temperature = 1878 C
Ramping rate increased to 1A/min for the TBHT.
Tapped manually to 454 A, Temperature 1880 C.
Saturday, October 27 2018, 10:00
Ramping down to 0 A @ 2 A/min.
Monday, October 29, 2018, 12:39
Venting EVAP2, TaC coat sintering completed. |
Tuesday, September 11, 2018, 10:47, Aaron Schmidt, , , , , Evap 2 step discrepancy
|
Tuesday, September 11, 2018, 10:45:
TGHT: 53.4 A TBHT: 57.75
Actual
TGHT: 60.0A TBHT: 59.0A
Uploaded the rest to Word doc. Screenshots included. |
Monday, September 10, 2018, 15:09, Marla Cervantes, Empty, 42218-3, LP-IG-LIS, Done, TaC coating/sintering for UC target container
|
Monday, September 10, 2018, 15:09
Container is coated with TaC and wrapped with Ta heat-shield ( 3 layers)
Desired temp = 1900 C (expected TGHT ~445A/7.5V), TBHT will be set fixed at 230A (max).
Good vac at 3.00-5 Torr
Bad vac at 5.0e-5 Torr.
Chamber is currently being pumped down
Tuesday, September 11, 2018, 09:27
Pressure at IGP1 8.61e-7 Torr.
Auto ramping TGHT at 1A/min to reach 400A, and TBHT at 1A/min to reach 230A.
Tuesday, September 11, 2018, 12:05
Pressure increased to 6.9e-e5 Torr and auto-ramp reduced the current:
TGHT from 94.6 A to 84.86 A
TBHT from 87.8 A to 78.87 A
(see figure EVAP2-_01)
EPICS automatically started ramping up TBHT and TGHT current when the pressure was between the good limit.
Tuesday, September 11, 2018, 14:29
TBHT current reached ~230 A and EPICS stopped inputting current automatically.
TBHT current reading on:
EPICS 232.8 A
Power supply: 235 A
Tuesday, September 11, 2018, 16:53
TGHT reached 400 A, EPICS stopped auto-ramping automatically. (Fig. Heater-ramp and Plot_400A-230A)
Temperature read by OMEGA 1837 C (Fig. Tempeature-at-400A)
Tuesday, September 11, 2018, 17:40
TGHT current was increased manually to 419 A (power supply current 422 A, EPICS plot 421.6 A) in steps of ~5A/2min
The temperature after ~30 min of being at 419 A is 1898 C.
The container will stay 5 hours at 1898 C
Wednesday, September 12, 2018, 09:05
EVAP2 remained at max setpoints for 5hrs
Auto-cool was set to 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
The automatic ramp decreased the TBHT current to 0A, but not so for TGHT,
TGHT only reduced to 22 A, the TGHT was manually tapped to 0A
Wednesday, September 12, 2018, 18:30
Process completed (fig. TaC-coating).
Chamber was vented. |
Tuesday, September 04, 2018, 17:04, John Wong, Empty, , LP-SIS, Problems, TaC coating/sintering for UC target container
|
Tuesday, September 04, 2018, 16:58
Container is coated with TaC and wrapped with Ta heat-shield ( 3 layers)
Desired temp = 1900 C (expected TGHT ~445A/7.5V), TBHT will be set fixed at 230A (max).
Good vac at 3.00-5 Torr
Bad vac at 5.0e-5 Torr.
Chamber is currently being pumped down
Wednesday, September 05, 2018, 10:53
Pressure at 9.5-7 Torr.
Auto ramping TGHT at 1A/min to reach 400A, and TBHT at 1A/min to reach 230A.
Wednesday, September 05, 2018, 17:52
Problem with TGHT readback vs setpoint. TGHT ramped up to 400A, temp measured at 1830C. However, the setup remained at 228A (see attachment). The autoramping program only sees the readback; in this case, the TGHT would continue to keep ramping up until the target breaks. The autoramping program has stopped just in time.
TGHT stepped down to 400A (setpoint), readback at 206A/6.59V. TGHT at 230A/4.16V. Temperature holding at 1783C.
Control has been informed.
Thursday, September 06, 2018, 10:54
Target temp holding at 1773C. Pressure at 8.5e-7 Torr.
Ramping down TGHT and TBHT, and inspect the container later.
Problem with the TGHT readback/setpoint will need to be investigated.
Friday, September 07, 2018, 16:03
Target container is nicely sintered.
Awaiting for Control group to investigate with the problem on TGHT readback/setpoint.
|
Monday, August 20, 2018, 18:10, John Wong, np-SiC, 43044-1, LP-SIS, Done, nano-SiC final conditioning
|
Monday, August 20, 2018, 17:58
14.9 g of np-SiC fibrous target discs are loaded into the container (previously coated with TaC and sintered, see elog ID 414).
Total loaded length 9.5 cm.
A 1.5" width graphite sheet is used as under layer to prevent TaC diffused to the discs; this was observed during the heat treatment, (see dropbox SEM images).
Both end caps are in. With ionizer pointing out, right cap is expended BUT NOT left cap - will need to expend this after the conditioning.
No Ta heat-shield is used.
Final conditioning temperature: 1500 C (As per e-log 414, TGHT = 450A/7.31V, 3.28kW)
Keeping TBHT at 0A for now - will ramp up after TGHT reach to the desired temperature.
OMEGA slope set at 0.99
Good vac = 3.0e-5 Torr,
Bad vac = 5.0e-5 Torr.
Tuesday, August 21, 2018, 10:24
Pressure at 1.2e-6 Torr.
Initiated autoramping at 2A/min for TGHT to reach 400A - monitoring temp and vacuum.
TBHT set at 10A.
Tuesday, August 21, 2018, 15:13
Temp reached to 1350C. TGHT at 400A/6.7V. Pressure at 1.9e-6 Torr after holding at the temp for 100 min.
Tuesday, August 21, 2018, 15:28
Tapped up TGHT to 450A/7.8V (3.5kW). Temp measured at 1465 +/- 5 C. Pressure coming down from 3.5 e-6 Torr.
Tuesday, August 21, 2018, 15:32
Tapping up TBHT to 230A
Tuesday, August 21, 2018, 16:25
TBHT at 230A/4.33V. Pressure started to increase from 150A, and reached to 3.3e-6 Torr after TGHT reached to the setting.
Temperature measured at 1475 C +/- 5C. Holding at this temperature until vacuum comes to stabilization (est.2-3 hours)
Tuesday, August 21, 2018, 16:45
Checked with Mikron (slope set at 0.99); temp on left end-cap measured at 1490 +/- 20C (that's close enough). Temp on ionizer tube about 1900C
Tuesday, August 21, 2018, 22:12
Pressure at 1.7e-6 Torr. Temp holding at 1480C, TGHT at 450/7.7V, TBHT 230A/4.27V.
Cooling down at 2A/min for TGHT and 1A/min for TBHT
|
Wednesday, July 25, 2018, 17:33, John Wong, Empty, 43044-2, LP-SIS, Done, TaC coating/sintering for UCx#24
|
Wednesday, July 25, 2018, 17:32
Container is coated with TaC and wrapped with 3 layers of Ta heat-shields.
Desired sintering temperature ~1900 C, TGHT is estimated to be ~ 445A (3.3 kW), TBHT set to 230A (as usual).
OMEGA slope set to 0.99
Good vac = 3.0 e-5 Torr, Bad vac = 5.0 e-5 Torr.
Chamber is currently being pumped down.
Friday, July 27, 2018, 10:32
Vacuum at 9.9 e-7 Torr.
Autoramp TGHT at 1A/min to 300A and TBHT at 1A/min to 230A. Will monitor temp and adjust TGHT to reach the desire temp.
Friday, July 27, 2018, 16:31
TGHT reached to 1500 C, and TBHT at 230A, Temp at 1480 C, pressure at 2.e-6 Torr.
Autoramp TGHt at 1A/min to 400A. Continue monitoring temp.
Saturday, July 28, 2018, 12:41
TGHT at 400A/6.2V. Temp at 1730 C. Pressure 7.4 e-7 Torr.
Tapped up TGHT to 450A/7.2V, temp at 1891 C. Holding at this current... Pressure coming down from 1.2e-6 Torr.
Monday, July 30, 2018, 22:40
Target temp has been held at 1880 C, TGHT at 450A/7.57V, TBHT 230/4.18V, vaccum at 3.8 e-7 Torr.
Cooling TGHT and TBHT at 2A/min and 1A/min, respectively.
Tuesday, July 31, 2018, 10:23
TGHT/TBHT at 0A. Pressure at 1.5e-7 Torr.
Process completed.
Venting chamber.
Target containers looks good. Transferred to Ar glovebox.
|
Tuesday, July 10, 2018, 16:43, John Wong, Empty, , LP-SIS, Done, For nano-SiC#1
|
Tuesday, July 10, 2018, 16:40
Container was flashed with TaC solution and let dry in air.
No Ta heat shield is used.
Desired temperature 1900C, ramp up TGHT accordingly. (Take note at 1500 and 1600 C).
OMEGA slope setting = 0.98
TBHT set at 250A (as usual)
Chamber is currently being pump down.
Wednesday, July 11, 2018, 10:54
Pressure at 4.5 e-7 Torr.
Autoramping TGHT at 0.1A/min to reach 300A and TBHT at 0.1A/min to reach 230A.
Once TGHT setting is reached, it will be further increased according to the temp measurement.
Friday, July 13, 2018, 10:57
TGHT at 300A/4.02V but temp is still too low to be detected.
Increase TGHT to 400A, ramping at 1A/min. TBHT is already at 230A/4.0V.
Current pressure at 4.4e-7 Torr.
Friday, July 13, 2018, 13:09
TGHT reached 400A/5.85V, temp reading 1112C.
Ramping up to 500A
TGHT reached 500A/7.9V. temp reading 1250 C.
Ramping up to 600A
Friday, July 13, 2018, 17:13
TGHT reached 600A/10.74V, temp reading 1742 C.
Ramping up to 650A
Wednesday, July 18, 2018, 11:54
TGHT has remained at 650A/12.05V since Friday July 13.
Temperature check:
pyrometer: 1650 (250 correction) = 1900 C
OMEGA: 1-color (e= 0.32 for spectral hemispherical) = 1910 C
OMEGA: 2-color (slope @ 0.99) = 1905 C
Measurements are in agreement
Cooling TGHT at 2A/min, TBHT at 1A/min. Current pressure 3.7e-7 Torr.
Wednesday, July 18, 2018, 13:47
TGHT at 500A, 8.4V, temp at 1600 C (4.2 kW)
TGHT at 475/7.84V, temp at 1550 C (3.72 kW - Max operating target heating power)
TGHT at 450/7.31V, temp at 1500 C (3.28 kW)
With TBHT set for 230A, usual operation setting, the temperature on the transfer tube is to exceed 2000 C. Keeping TBHT at that setting may affect the overall temperature.
Note: To condition the nanoSiC, it is better to keep TBHT at 0A and ramp up TGHT to 475A while monitoring the vacuum. Then step up TBHT; any increase in vacuum would indicate a local evaporation of nanoSiC close to the ionizer.
Temp measurement is complete, cooling down TGHT/TBHT to zero.
Thursday, July 19, 2018, 12:23
TGHT has been at 0A for over 18 hours. Vacuum pressure at 7e-8 Torr.
Venting chamber.
|
Tuesday, July 03, 2018, 17:05, John Wong, np-SiC, Tube container, , Done, NanoSiC thermal treatment batch #3
|
Tuesday, July 03, 2018, 17:02
49 discs/ 15.42g np-SiC fibrous discs loaded into the tube container
Heat treatment is similar to previous process, see elog#408/409.
TGHt should be set at 330A/5.2V to reach temp 1575C (+/- 25C)
Omega slope set at 1.05 (for carbide)
Chamber is currently being pumped down
Wednesday, July 04, 2018, 10:38
Pressure at 1.5 e-6 Torr.
Initiated auto-ramping at 0.2A/min to reach 330A/5.2V.
Monday, July 09, 2018, 14:44
TGHT has been stabilized at 330A/5.2V for 24 hours. Pressure at 3.7e-7 Torr.
Temp was measured at 1400C - light coating on window likely affected the measurements.
Measured with one-color pyrometer on Ta body inside the target container = 1550 C (with the correction of 250C for Ta).
Adjusted OMEGA slope to 1.18, temp currently at 1580 C.
Monday, July 09, 2018, 16:42
Pressure stabilized at 3.5e-7 Torr.
Initiated auto-cooling at 1A/min.
Tuesday, July 10, 2018, 11:11
Target is at room temperature.
Process completed; see attachment for the data retrieval and dropbox (np-SiC production folder) for screen capture.
mass loss = (15.42 - 8.09) g = 7..33 g (47.5%) [in agreement - good!]
|
Thursday, June 21, 2018, 11:38, Aaron Schmidt, Ta, 42218-9, HP-SIS, Done, Conditioning Ta#56
|
Ta#56 HP-SIS target description:
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.025mm
Target density = 14.01 g/cm3
Target length = 3.4 cm
Total Mass = 47.374 g [Incl foils + Ta wire on 6 packs]
Total mass w/ Target oven= 1469 g
Discs in target are arranged as follows: 1pack / 75singles / 1pack / 100singles / 2packs / 100singles / 1pack / 75singles / 1pack
Thursday, June 21, 2018, 11:430: Ta#56 loaded into Evap 2
Thursday, June 21, 2018, 11:37: Roughing
Thursday, June 21, 2018, 11:48 : Turbo pump started.
Thursday, June 21, 2018, 11:56 : Turbo pump at speed
Monday, June 25, 2018, 08:00: Vacuum @ 3.35e-07T
Monday, June 25, 2018, 08:05: TGHT/TBHT Power supplies switched on.
Monday, June 25, 2018, 09:35: Vacuum @ 3.23e-07T. Manually bump up TGHT to 40A.
Slope found / set.
TBHT will be ramped up to 230A at 1.0A/min.
TGHT will be ramped up to 650A at 2.0A/min.
Final desired temperature = 1900C
OMEGA slope = 0.98
Monday, June 25, 2018, 11:41: Auto-ramping TGHT / TBHT @ 2 / 1 A per min to 300 / 180 A
Monday, June 25, 2018, 13:28: Check: Vacuum @ 1.08e-06T. TGHT / TBHT @ 248 / 110 A
Monday, June 25, 2018, 13:50: TGHT ramping halted momentarily. Limit increased to 350 A, continue ramping.
Monday, June 25, 2018, 14:44: Check: Vacuum @ 1.08e-06T. TGHT / TBHT @ 350 / 180 A. (hold till am)
Omega: 1033 deg C
Tuesday, June 26, 2018, 08:37: Vacuum @ 3.03e-07T. Auto-ramping TGHT / TBHT @ 2 / 1 A per min to 600 / 230 A . Omega: 1010 deg C (approx)
Tuesday, June 26, 2018, 11:25: Vacuum @ 1.34e-06T. TGHT / TBHT @ 248 / 110 A. Omega: 1605 deg C (approx)
Auto-ramping TGHT @ 2 A per min to 650 A
Tuesday, June 26, 2018, 12:06: Limited at 608A ? Display still ramping past the auto-ramp limit.
Tuesday, June 26, 2018, 12:24 : Auto ramp halted. Display brought to 610 A. Readback 603 A
Tuesday, June 26, 2018, 12:41: Voltage limit adjusted to 12.00V. Mnaualy increased TGHT to 620 A. Auto-ramping TGHT @ 2 A per min to 650 A
Tuesday, June 26, 2018, 12:59: Check: Vacuum @ 1.53e-06T. TGHT / TBHT @ 650 / 230 A.
Omega: 1747 deg C
Tuesday, June 26, 2018, 15:07: Check: Vacuum @ 9.73e-07T. TGHT / TBHT @ 650 / 230 A. (hold till am)
Omega: 1760 deg C
Wednesday, June 27, 2018, 07:49: Check: Vacuum @ 5.06e-07T. TGHT / TBHT @ 650 / 230 A.
Omega: 1796 deg C. Begin auto-ramping TGHT to 700 A @ 2 A per min with pause at 675 A. Monitor.
Wednesday, June 27, 2018, 08:00: Check: Vacuum @ 5.80e-07T. TGHT / TBHT @ 675 / 230 A.
Omega: 1843 deg C. Begin auto-ramping TGHT to 700 A @ 2 A per min. Monitor.
Wednesday, June 27, 2018, 08:16: Vacuum @ 7.45e-07T. TGHT / TBHT @ 700 / 230 A. Omega: 1890 deg C (approx).
Wednesday, June 27, 2018, 08:23: Vacuum @ 8.53e-07T. TGHT / TBHT @ 707 / 230 A. TGHT Voltage= 10.783V. Omega: 1906-1913 deg C. Desired temperature = 1900C reached.
Wednesday, June 27, 2018, 13:11: Vacuum @ 6.77e-07T. Omega: 1902-1915 deg C
Wednesday, June 27, 2018, 14:53: Begin auto-cooling TGHT / TBHT @ - 2 / -1 A per min overnight.
Thursday, June 28, 2018, 07:39: Power supplies off. Turbo pump off.
Thursday, June 28, 2018, 09:38: Vented. Remove From Evap 2. |
Friday, June 08, 2018, 08:33, Aaron Schmidt, , , , Problems resolved, Chiller tripped / Alarm
|
Alarm noted on passing Hot Lab. RPG notified, no radiological hazards. ISAC ops contacted, drop in DI water last night.
Entered w/ PPE. Chiller alarming. Evap 1 running ok
Friday, June 08, 2018, 08:30: Chiller turned on/off. Reset. No alarm. |
Wednesday, May 23, 2018, 15:21, Laura Lambert, Empty, , HP-FEBIAD-CTL, Done, Sintering TaC coating container for UCx#23
|
Wednesday, May 16, 2018, 09:56
Container coated with TaC using 'flushing technique' and let dry over weekend.
Cleaned ionizer tube with acetone, no coating inside ionizer tube.
Wrapped with 3 x Ta heat shields, not incl center block
OMEGA slope = 0.98
*NOTE: realized after pumping down, filament on IGP2 is burnt out and needs replacing, will order a new one and use IGP1 for this process
Thursday, May 17, 2018, 13:15
HS water valves remained open since the last time evap2 was used, no leak check done.
Tapped up manually to 50A.
Waited ~1hr
Vacuum stable.
IGP1 = 1e-6 Torr
Initiating auto ramp for TGHT @ 0.2A/min to a max setpoint of 350A
Initiating auto ramp for TBHT @ 0.1A/min to a max setpoint of 230A
Once max setpoints achieved, will tap up manually to final desired temperature of 1900C
Friday, May 18, 2018, 13:00
Tapped up manually.
TGHT = 495A, 8.84V
TBHT = 230A, 3.26V
MIKRON = 2000C
Filament = 1910C
OMEGA = 1910C
Will remain at max setpoints over weekend.
Tuesday, May 22, 2018, 10:04
Remained at max setpoints over long wknd.
TGHT = 495A, 8.85V
TBHT = 230A, 3.26V
IGP1 = 2.47e-7 Torr
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Wednesday, May 23, 2018, 10:08
Vented in air this morning.
Container looks good!
Transferred into glove box.
|
Tuesday, May 08, 2018, 15:06, John Wong, np-SiC, Tube container , , Done, NanoSiC thermal treatment batch#2
|
Tuesday, May 08, 2018, 15:02
22 np-SiC fibrous discs loaded in the tube container (coated and sintered with TaC)
Heat treatment is similar to previous process, see elog #408.
TGHT should be set at 330A/5.2V to reach temp 1575C (+/- 25).
Omega slope set at 1.05 (for carbide)
Chamber is currently being pumped down
Tuesday, May 08, 2018, 22:46
Pressure at 2.2e-6 Torr.
Initiated autoramping at 0.2A/min to reach 330A
Friday, May 11, 2018, 11:11
TGHT reached to 330A/5.1V but temp was measured at 1400A; It was held at that current for about 10 hours.
Increased TGHT to 335A/5.2V - temp is holding at 1420C (Will check the window if there is any coating that might have caused the discrepancy)
Sunday, May 13, 2018, 00:25
In fact, the window is slightly coated. The temperature should already be at optimum, 1600C. Will keep heating for another day.
Sunday, May 13, 2018, 14:10
Temp holding up well.. Pressure at 1.8e-7 torr.
cooling down at 2A/min.
Monday, May 14, 2018, 09:33
Target has been cooled for over 18 hours. Pressure at 1.1e-7 Torr.
Venting chamber.
mass loss = (8.65 - 4.32)g = 4.33 g (50%) [slightly higher than expected, likely due to increase of 5A on TGHT]
|
Tuesday, May 01, 2018, 18:07, John Wong, np-SiC, Tube container, , Done, NanoSiC thermal treatment batch#1
|
Tuesday, May 01, 2018, 18:06
21 fibrous discs of nanoSiC are loaded into a tube container (coated/Sintered with TaC).
Thermal treatment temperature at 1600C, TGHT is ~338A/5.5V, according to elog #407.
Wednesday, May 02, 2018, 08:27
20 mins ago... initiate auto ramping at 0.2A to reach TGHT 250A. Instead of ramping incrementally, TGHT jumped straight to 250A; vacuum shot up to milli torr.
Turn off TGHT immediately to let vacuum stable down to 10-6 Torr.
System problem?? Archive striptool for more details.
Re-activate auto-ramping - OK!
Once TGHT reached 250A (18 hours later from now), will continue ramping up to reach 1600C
Friday, May 04, 2018, 01:09
TGHT just reach 250A, temp at about 1190C. Pressure remained high at 4.2e-5 Torr.
Continue autoramping to reach TGHT 300A.
Friday, May 04, 2018, 11:07
TGHT at 300A for about 1.5 hr. Temp at 1315C. Pressure at 5.7e-6 Torr.
Autoramp to 320A.
Friday, May 04, 2018, 14:39
Tapping up to 330A; temp at 1560C with slope changed to 1.05 (for carbide material). Will keep at this current/temp.
Sunday, May 06, 2018, 13:25
TGHT at 330A/5.2V; holding temp at 1550C. No coating on windows. Pressure at 1.6e-7 Torr.
Cooling down at 2A/min.
Monday, May 07, 2018, 10:49
Evap cooled. Venting chamber.
Inspection of the discs next...
mass loss = 6.79 - 3.62 = 3.1 g (46%) [in agreement, good]
|
Saturday, April 28, 2018, 16:12, John Wong, Empty, Tube container , , Done, TaC coating/sintering of Tube container
|
Saturday, April 28, 2018, 16:09
Container is coated with TaC and wrapped with TaC heatshield.
Will be used for carbonizing nanoSiC target materials.
Chamber is pumping down...
Sintering temp 1800C, est TGHT ~550A
Saturday, April 28, 2018, 18:08
Pressure at 5.e-6 Torr.
Initial auto-ramp at 1.0A/min reaching TGHT 500A. Monitoring temp.
Sunday, April 29, 2018, 23:37
Target temp stabilizes at 1800C with TGHT holding at 400A/7.02V for 24 hours. Pressure at 4.4 e-7 Torr.
Lower TGHT to 338A/5.51V to reach 1600C - This will temp/current will be used for carbonizing the nanoSiC fibers.
Holding TGHT overnight to determine temp stability.
Monday, April 30, 2018, 18:04
Temp is holding at 1600C, TGHT 338A/5.5V. Pressure at 3.0 e-7 Torr.
Initiated cooling down at 2A/min.
|
Wednesday, April 25, 2018, 07:21, Aaron Schmidt, , , , Done, HS swap evap 2
|
Wednesday, April 25, 2018, 07:05: TGHT & TBHT off
Wednesday, April 25, 2018, 07:15: BV1 & TP1 off
Wednesday, April 25, 2018, 07:17: PV1 & BP1off
Wednesday, April 25, 2018, 07:19: Begin venting
Wednesday, April 25, 2018, 07:22: Full venting.
Wednesday, April 25, 2018, 07:29: HS waterlines purged.
Wednesday, April 25, 2018, 07:48: Aurelia's test ta target assembly was removed. The blank target heating heat shield for evap 2 was reinstalled. shields in but empty.
Evap 2 Doors closed. |
Thursday, April 19, 2018, 12:38, Laura Lambert, Ta, 41177-3, LP-SIS, Done, Round 2. Temp measurements for Aurelia target Ta#56
|
Thursday, April 19, 2018, 12:37
See elog i.d. 404 for target description and first round of heating.
Endcaps inserted and expanded.
No Rh foil inserted.
Loaded into evap2 and chamber currently pumping down.
Thursday, April 19, 2018, 14:00: water cooling lines opened. No response. Vacuum @ 1.8e-06T - AS
Thursday, April 19, 2018, 14:07: Power supplies swtiched on. - AS |
Tuesday, April 17, 2018, 10:24, Laura Lambert, Ta, 41177-3, LP-SIS, Done, Conditioning Ta#56 back-up target/ Temp measurements for Aurelia
|
Tuesday, April 17, 2018, 10:20
Target consists of 470 discs.
Total packed length 3.4cm [exactly 7.8cm space on both sides]
Total mass g [Incl foils + Ta wire on 6 packs]
Target consists of 350 single discs and 6x20 packs of Ta discs
Discs in target are arranged as follows: 1pack / 75singles / 1pack / 100singles / 2packs / 100singles / 1pack / 75singles / 1pack
No Heat shields.
No endcaps inserted, no Rh foil inserted.
Chamber pumped down over night.
HS water valves opened, no leaks detected
Tapped up manually to 35A
Vacuum stable, IGP1 = 6.5e-7 Torr
Initiating auto-ramp.
OMEGA slope = 0.98
TGHT will be ramped up to 300A at 1.0A/min.
Aurelia will take over for temp measurements.
Final desired temperature = 1900C
Vacuum limit stop at 3.0e-5 Torr, backing off at 8.0e-5 Torr.
Thursday, April 19, 2018, 08:39
First round of temperature measurements complete.
Reached a max current of 600A, ~1700C
Cooled down overnight.
Will remove from evap2, insert endcaps, and load back in for more measurements.
Thursday, April 19, 2018, 12:35
Vented in air and removed from evap2.
See next elog for follow up temperature measurements.
|
Thursday, March 08, 2018, 11:05, Marla Cervantes, Empty, 39530-3, LP-FEBIAD, Done, Temperature measurements for ARIEL
|
Friday, March 09, 2018, 11:03
LP-FEBIAD loaded into evap2 and pumped down.
Temperature measurements of the ionizer will be done by Fernando for ARIEL development.
Ta foil covering side holes on heat shield so no temp measurements can be done using OMEGA on side ports of evaporator as per request of Fernando
No Ta heat shields on container.
HS water valves opened, no leaks detected.
IGP1 = 1.72e-7 Torr
IGP2 = 1.36e-7 Torr
Tapped up to TGHT = 50 A, 0.54 V; TBHT = 50 A, 0.45 V
IGP1 = 1.8e-6 Torr
IGP2 = 1.4e-6 Torr
Initiating auto ramp for TGHT at 2.0A/min up to 310A and TBHT at 1.0A/min up to 210A
Monday, March 12, 2018, 10:16
IGP1 = 8.8e-8 Torr
IGP2 = 6.6e-8 Torr
TGHT = 310A, 5.06V
TBHT = 210A, 2.98 V
TGHT and TBHT will be adjusted accordingly for temperature measurements
Tuesday, March 13, 2018, 16:00
Temperature measurements done.
Initiated auto-cool.
TGHT cooling at 2.0A/min and TBHT at 1.0A/min.
Wednesday, March 14, 2018, 16:03
Removed from evap2. |
Wednesday, February 28, 2018, 15:18, Laura Lambert, Empty, 42218-13, LP-SIS, Done, Sintering TaC coating on UCx#22 container
|
Wednesday, February 28, 2018, 15:16
Container coated with TaC using 'flushing technique' and let dry.
Q-tip to plug ionizer became stuck in ionizer, removed manually with small drill bit.
Inspected ionizer with microscope, ionizer still good.
Cleaned ionizer tube with acetone.
Wrapped with 3 x Ta heat shields, incl center block
Currently pumping down in evap2
OMEGA slope = 0.98
Good vac at 3.0e-5, bad vac at 8.0e-5 Torr.
Thursday, March 01, 2018, 10:06
HW water valves opened yesterday, no leaks detected.
IGP1 = 2.8e-7 Torr
Tapped up manually to 40A.
Waited ~3hrs
Vacuum stable.
IGP1 = 5.3e-7 Torr
IGP2 = 5.4e-7 Torr
Initiating auto ramp for TGHT @ 1.0A/min to a max setpoint of 350A
Initiating auto ramp for TBHT @ 0.5A/min to a max setpoint of 230A
Once max setpoints achieved, will tap up manually to final desired temperature of 1900C
Thursday, March 01, 2018, 14:39
Vacuum started to climb very fast - auto-ramp was stopped.
Vacuum climbed up to IGP1 = 1.3e-4 Torr
Tapped TGHT back down to 80A from 90A, TBHT down to 50A from 60A.
Waited ~40min.
Vacuum stable, IGP1 = 2.6e-6 Torr
Restarting auto-ramp.
Thursday, March 01, 2018, 14:54
IGP1 = 2.1e-5 Torr
Vacuum climbing quite rapidly again, stopped auto-ramp and vacuum started to drop right away.
TGHT = 100A
TBHT = 56A
Waited ~10min
IGP1 = 6.0e-6 Torr
IGP2 = 5.2e-6 Torr
Decreasing ramping rate to 0.5A/min and 0.2A/min for the TGHT and TBHT respectively, and re-initiating auto-ramp.
Friday, March 02, 2018, 10:18
TGHT = 350A, 5.61V
TBHT = 230A, 4.04V
IGP1 = 4.3e-7 Torr
IGP2 = 3.8e-7 Torr
OMEGA = 1624C
Vacuum stable.
Increasing max setpoint of TGHT to 400A
Re-initiating auto-ramp of TGHT.
Friday, March 02, 2018, 11:04
TGHT = 372A, 6.05V
IGP1 = 5.0e-7 Torr
Increasing ramping rate for TGHT to 1.0A/min
Friday, March 02, 2018, 11:44
TGHT = 400A, 6.60V
IGP1 = 6.9e-7 Torr
OMEGA = 1780C
Vacuum stable.
Increasing max setpoint of TGHT to 430A
Re-initiating auto-ramp of TGHT.
Friday, March 02, 2018, 12:17
TGHT = 430A, 7.22V
OMEGA = 1866C
IGP1 = 9.5e-7 Torr
Tapped up manually to OMEGA = 1910C
TGHT = 445A, 7.57V
TBHT = 230A, 4.07V
IGP1 = 1.1e-6 Torr
IGP2 = 9.9e-7 Torr
Monday, March 05, 2018, 08:41
Remained at max setpoints over the weekend.
TGHT = 445A, 7.47V
TBHT = 230A, 4.06V
IGP1 = 1.87e-7 Torr
IGP2 = 1.47e-7 Torr
OMEGA = 1894C
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Tuesday, March 20, 2018, 14:53
Vented in air.
Container was transferred to glove box for loading ~1 week ago
Container looks good.
|
Monday, February 19, 2018, 14:16, Laura Lambert, Empty, 39530-3, LP-FEBIAD, Done, Temperature measurements for ARIEL
|
Monday, February 19, 2018, 13:39
LP-FEBIAD loaded into evap2 this morning and pumped down.
Temperature measurements of the ionizer will be done by Fernando for ARIEL development.
Ta foil covering side holes on heat shield so no temp measurements can be done using OMEGA on side ports of evaporator as per request of Fernando
No Ta heat shields on container.
HS water valves opened, no leaks detected.
IGP1 = 2.75e-6 Torr
IGP2 = 1.42e-6 Torr
Tapped up to TGHT = 50A, 0.53V; TBHT = 50A, 0.56V
IGP1 = 2.64e-6 Torr
IGP2 = 1.35e-6 Torr
Initiating auto ramp for TGHT at 2.0A/min up to 350A and TBHT at 1.0A/min up to 210A
Tuesday, February 20, 2018, 09:15
IGP1 = 6.9e-7 Torr
IGP2 = 3.8e-7 Torr
TGHT = 350A, 5.98V
TBHT = 210A, 3.02V
TGHT and TBHT will be adjusted accordingly for temperature measurements...
Tuesday, February 27, 2018, 14:55
Temperature measurements done.
Initiated auto-cool.
TGHT cooling at 2.0A/min and TBHT at 1.0A/min.
Wednesday, February 28, 2018, 10:39
Tuesday, December 19, 2017, 11:40
Vented in air and removed from evap2 today.
|
Wednesday, December 13, 2017, 10:55, Laura Lambert, Empty, 39530-3, LP-FEBIAD, Done, Temperature measurements for ARIEL
|
Wednesday, December 13, 2017, 10:36
LP-FEBIAD loaded into evap2 this morning and pumped down.
Temperature measurements of the ionizer will be done by Fernando for ARIEL development.
Ta foil covering side holes on heat shield so no temp measurements can be done using OMEGA on side ports of evaporator as per request of Fernando
No Ta heat shields on container.
HS water valves opened, no leaks detected.
IGP1 = 2.3e-6 Torr
IGP2 = 1.7e-6 Torr
Tapped up to TGHT = 50A, 0.30V; TBHT = 50A, 0.59V
IGP1 = 1.8e-6 Torr
IGP2 = 1.4e-6 Torr
Initiating auto ramp for TGHT at 2.0A/min up to 350A and TBHT at 1.0A/min up to 210A
Wednesday, December 13, 2017, 14:53
IGP1 = 7.6e-7 Torr
IGP2 = 6.4e-7 Torr
TGHT = 350A, 5.85V
TBHT = 210A, 3.02V
TGHT and TBHT will be adjusted accordingly for temperature measurements...
Thursday, December 14, 2017, 09:16
IGP1 = 2.1e-7 Torr
IGP2 = 1.7e-7 Torr
TGHT = 385A, 6.80V
TBHT = 210A, 3.01V
Tapped up to TGHT = 400A, 7.11V
Stopped for temperature measurements.
Tapped up to TGHT = 450A, 8.20V
Friday, December 15, 2017, 09:50
IGP1 = 1.2e-7 Torr
IGP2 = 9.6e-8 Torr
TGHT = 350A, 5.82V
TBHT = 210A, 2.94V
Initiating auto-ramp to TGHT = 650A
Monday, December 18, 2017, 10:43
Temperature measurements done.
Initiated auto-cool.
TGHT cooling at 2.0A/min and TBHT at 1.0A/min.
Tuesday, December 19, 2017, 11:40
Vented in air and removed from evap2 today.
|
Monday, December 11, 2017, 14:22, Laura Lambert, , , , Maintenance, Interlock limits updated to 500mTorr
|
Monday, December 11, 2017, 14:21
Dave updated evap2 interlock limits to 500mTorr for TGHT and TBHT on friday
|
Thursday, December 07, 2017, 10:03, Laura Lambert, Endcaps, , TARGET BOAT, In progress, Sintering TaC coating on endcaps and springs
|
Thursday, December 07, 2017, 09:57
Each endcap is wrapped in a separate piece of graphite foil and placed in a target boat.
There are also 4 coated springs, 2 on each side of the stack of endcaps.
The boat is wrapped with 3-layers of Ta heatshields.
Chamber pumped down overnight.
OMEGA slope = 0.98
HS water valves opened, no leaks detected.
IGP1 = 5.9e-7 Torr
IGP2 = 4.0e-7 Torr
Tapping up manually.
Final desired temperature = 1800C
|
Thursday, December 07, 2017, 11:56, Laura Lambert, Endcaps, , TARGET BOAT, Problems, Sintering TaC coating on endcaps and springs
|
Laura Lambert wrote: |
Thursday, December 07, 2017, 09:57
Each endcap is wrapped in a separate piece of graphite foil and placed in a target boat.
There are also 4 coated springs, 2 on each side of the stack of endcaps.
The boat is wrapped with 3-layers of Ta heatshields.
Chamber pumped down overnight.
OMEGA slope = 0.98
HS water valves opened, no leaks detected.
IGP1 = 5.9e-7 Torr
IGP2 = 4.0e-7 Torr
Tapping up manually.
Final desired temperature = 1800C
|
Thursday, December 07, 2017, 11:51
TGHT tripped off.
Turns out the vacuum limits have not been fully updated when they should have been and the old ones still apply.
IGP1 reached 8e-5 Torr which tripped off the system.
TGHT = 80A, 1.05V when the system tripped.
|
Friday, December 08, 2017, 15:29, Laura Lambert, Endcaps, , TARGET BOAT, Problems resolved, Sintering TaC coating on endcaps and springs
|
Laura Lambert wrote: |
Laura Lambert wrote: |
Thursday, December 07, 2017, 09:57
Each endcap is wrapped in a separate piece of graphite foil and placed in a target boat.
There are also 4 coated springs, 2 on each side of the stack of endcaps.
The boat is wrapped with 3-layers of Ta heatshields.
Chamber pumped down overnight.
OMEGA slope = 0.98
HS water valves opened, no leaks detected.
IGP1 = 5.9e-7 Torr
IGP2 = 4.0e-7 Torr
Tapping up manually.
Final desired temperature = 1800C
|
Thursday, December 07, 2017, 11:51
TGHT tripped off.
Turns out the vacuum limits have not been fully updated when they should have been and the old ones still apply.
IGP1 reached 8e-5 Torr which tripped off the system.
TGHT = 80A, 1.05V when the system tripped.
|
Friday, December 08, 2017, 15:29
Interlocks have been updated.
TGHT should now run up to 500mTorr before tripping off.
|
Friday, December 08, 2017, 15:42, Laura Lambert, Endcaps, , TARGET BOAT, Done, Sintering TaC coating on endcaps and springs
|
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Thursday, December 07, 2017, 09:57
Each endcap is wrapped in a separate piece of graphite foil and placed in a target boat.
There are also 4 coated springs, 2 on each side of the stack of endcaps.
The boat is wrapped with 3-layers of Ta heatshields.
Chamber pumped down overnight.
OMEGA slope = 0.98
HS water valves opened, no leaks detected.
IGP1 = 5.9e-7 Torr
IGP2 = 4.0e-7 Torr
Tapping up manually.
Final desired temperature = 1800C
|
Thursday, December 07, 2017, 11:51
TGHT tripped off.
Turns out the vacuum limits have not been fully updated when they should have been and the old ones still apply.
IGP1 reached 8e-5 Torr which tripped off the system.
TGHT = 80A, 1.05V when the system tripped.
|
Friday, December 08, 2017, 15:29
Interlocks have been updated.
TGHT should now run up to 500mTorr before tripping off.
|
Friday, December 08, 2017, 15:41
IGP1 = 2.8e-7 Torr
IGP2 = 1.9e-7 Torr
Tapped up manually to 50A
Initiated auto-ramp at a rate of 0.2A/min up to 300A.
Vacuum limit stop at 3.0e-5 Torr, backing off at 4.0e-5 Torr.
Monday, December 11, 2017, 09:37
IGP1 = 2.4e-7
TGHT = 300A, 4.80V
OMEGA = 1175C
Tapping up manually...
Monday, December 11, 2017, 14:19
Tapped up manually to 1800C
IGP1 = 2.1e-6 Torr
IGP2 = 2.1e-6 Torr
TGHT = 545A, 9.90V
OMEGA = 1810C
Will remain at max setpoints overnight and cool down in the a.m.
Tuesday, December 12, 2017, 09:01
TGHT = 545A, 9.96V
OMEGA = 1833C
Remained at max setpoints for ~18hrs
IGP1 = 4.2e-7 Torr
IGP2 = 3.9e-7 Torr
Initiating auto-cool at 2.0A/min
Wednesday, December 13, 2017, 11:05
Vented in air and removed from evap2 this morning.
|
Wednesday, November 29, 2017, 16:18, Laura Lambert, Empty, 39530-3, LP-FEBIAD, Done, Temperature measurements for ARIEL
|
Wednesday, November 29, 2017, 16:17
LP-FEBIAD loaded into evap2 today and currently pumping down.
Temperature measurements of the ionizer will be done by Fernando for ARIEL development.
Ta foil covering side holes on heat shield so no temp measurements can be done using OMEGA on side ports of evaporator as per request of Fernando
No Ta heat shields on container.
Final desired temperature of ionizer = 2000C
Thursday, November 30, 2017, 09:51
HS water valves opened, no leaks detected.
IGP1 = 2.1e-7 Torr
IGP2 = 1.7e-7 Torr
Tapped up to TGHT = 350A, 5.83V; TBHT = 230A, 3.31V
IGP1 = 6.3e-7 Torr
IGP2 = 3.7e-7 Torr
Will check temp measurements in lab after lunch before proceeding...
Friday, December 01, 2017, 11:04
Temperature measurements done.
Initiated auto-cool this morning.
TGHT cooling at 2.0A/min and TBHT at 1.0A/min.
Monday, December 04, 2017, 11:04
Removed from evap2 this morning. |
Thursday, November 23, 2017, 15:10, Laura Lambert, , 41882-4, TARGET BOAT, Done, Graphite insert test 6x
|
Thursday, November 23, 2017, 14:54
Graphite insert loaded into previously TaC coated target boat.
One endcap removed to allow for outgassing: left side out, right side in.
Weight of graphite tube + single endcap = 10.2012g
Same Ta heats shields remain on container from sintering TaC coating.
Currently pumping down in evap2.
Friday, November 24, 2017, 11:31
IGP1 = 4.52e-7 Torr
IGP2 = 3.43e-7 Torr
OMEGA slope = 0.98
Good vac at 3.0e-4, bad vac at 8.0e-4 Torr.
HS water valves have remained open since the last time evap2 was used.
No leak check done.
Tapped up manually to 50A.
Vacuum stable.
IGP1 = 5.34e-7 Torr
IGP2 = 5.54e-7 Torr
Initiating auto ramp for TGHT @ 0.2A/min to a max setpoint of 300A
Once max setpoints achieved, will tap up manually to final desired temperature of 2000C
Uranium targets go to a max temperature of 1950C online, so graphite insert should be tested to 2000C
Monday, November 27, 2017, 10:15
IGP1 = 2.5e-7 Torr
IGP2 = 1.9e-7 Torr
Reached 300A, 4.61V
OMEGA = 1298C
Tapped up manually to 485A, 8.46V
OMEGA = 1808C
Remained at this setpoint for a day
Tuesday, November 28, 2017, 15:41
IGP1 = 3.88e-7 Torr
IGP2 = 3.58e-7 Torr
Tapping up to 2000C...
Tuesday, November 28, 2017, 16:10
TGHT = 570A, 10.20V
OMEGA = 2005C
IGP1 = 9.64e-7 Torr
IGP2 = 1.05e-6 Torr
There was a minor drop in voltage at 540A, 9.58V - dropped to ~9.4V then slowly went back up to 9.58V [see photo]
Will remain at this setpoint overnight and cool down in the a.m.
Wednesday, November 29, 2017, 08:48
Voltage increased slowly while sitting at max setpoint of 570A [see photo]
TGHT = 570A, 11.20V --> voltage increased by 1.0V over ~16.5hrs
OMEGA = 2114C
IGP1 = 6.6e-7 Torr
IGP2 = 6.5e-7 Torr
Initiating auto-cool at 2.0A/min
Wednesday, November 29, 2017, 16:15
Vented in air and removed today.
Will update tomorrow with results and photos.
|
Tuesday, November 21, 2017, 13:55, Laura Lambert, Empty, 41882-4, TARGET BOAT, Done, Sintering TaC coating on fully enclosed target boat for graphite test
|
Tuesday, November 21, 2017, 12:01
Boat coated with TaC using 'flushing technique' and let dry overnight.
Wrapped with 1 long Ta heat shield 3x
Loaded into evap2 just before lunch
IGP1 = 7.1e-6 Torr
OMEGA slope = 0.98
Good vac at 3.0e-4, bad vac at 8.0e-4 Torr.
HS water valves have remained open since the last time evap2 was used.
No leak check done.
Tapped up manually to 35A.
Waited ~25min
Vacuum stable.
IGP1 = 1.15e-5 Torr
IGP2 = 1.17e-5 Torr
Initiating auto ramp for TGHT @ 0.2A/min to a max setpoint of 300A
Once max setpoints achieved, will tap up manually to final desired temperature of 1900C
Wednesday, November 22, 2017, 09:32
TGHT = 270A, 4.15V
OMEGA = 1285C
IGP1 = 1.23e-6 Torr
IGP2 = 1.13e-6 Torr
Vacuum stable.
Increasing ramping rate to 1.0A/min and final setpoint to 350A
Wednesday, November 22, 2017, 10:25
TGHT = 325A, 5.15V
OMEGA = 1500C
IGP1 = 2.80e-6 Torr
IGP2 = 2.93e-6 Torr
Vacuum stable.
Increasing ramping rate to 1.5A/min and final setpoint to 400A
Wednesday, November 22, 2017, 10:49
TGHT = 350A, 5.60V
OMEGA = 1580C
IGP1 = 4.5e-6 Torr
IGP2 = 4.9e-6 Torr
Vacuum stable.
Increasing ramping rate to 2.0A/min
Wednesday, November 22, 2017, 11:18
TGHT = 400A, 6.64V
OMEGA = 1734C
IGP1 = 5.8e-6 Torr
IGP2 = 6.2e-6 Torr
Vacuum stable.
Increasing final setpoint to 450A.
Wednesday, November 22, 2017, 15:59
TGHT = 460A, 8.07V
OMEGA = 1898C
IGP1 = 1.34e-6 Torr
IGP2 = 1.27e-6 Torr
Sintering process complete.
Remained at max setpoints for just over 4hrs.
Initiating auto-cool at 2.0A/min.
Thursday, November 23, 2017, 13:09
Removed from evap2 this morning.
Coating looks good.
|
Monday, November 06, 2017, 18:25, John Wong, np-SiC, , TARGET BOAT, Done, Thermal treatment npSiC Horn vs Probe samples - P74
|
Monday, November 06, 2017, 18:21
Samples of Horn and Probe - npSiC. see pg 74.
6 samples in total, to be heated to 1550C, about 450A. Set ramping rate at 0.2A/min.
Chamber pumping down
Tuesday, November 07, 2017, 15:01
TGHT reached to 450A/8.2V, temperature measured at 1460C. See attachment 1.
Increased ramping to 480A, targeting 1550C.
Tuesday, November 07, 2017, 22:26
Samples have been heating at 1550C with TGHT at 480A/8.78V for about 8 hours.
Vacuum stabilizes at 8.4e-7 Torr.
Initial cooling at 2A/min.
Wednesday, November 08, 2017, 10:36
Venting chamber.
|
Wednesday, October 04, 2017, 16:40, John Wong, np-SiC, , TARGET BOAT, Done, Thermal treatment cast-pellet npSiC/PAN - det. sintering effect
|
Wednesday, October 04, 2017, 16:37
3 samples of npSiC/PAN cast-pellets, see lab book p. 57 for details.
Desired temperature 1550C, expected TGHT ~450A.
Chamber pumped down.
TGHT ramping at 0.2A/min
Friday, October 06, 2017, 10:45
TGHt at 450A/7.7A, temp at 1510C. (p.s voltage is lower than before, elog 389).
Tapped up to 466A/8.08v, temp reached to 1550C. A slight increase in pressure when tapping up TGHT. (see attached screen capture)
Will maintain heating temperature for several days before cooling down
Tuesday, October 10, 2017, 10:50
Samples was heated for several days at 1550C.
Cooling down initiated at 2A/min.
Tuesday, October 10, 2017, 18:07
Chamber is vented.
Process done
|
Wednesday, September 27, 2017, 18:06, John Wong, np-SiC, , TARGET BOAT, Done, NS-npSiC & B3 pellets heat treatments
|
Wednesday, September 27, 2017, 18:05
3 samples from NS-npSiC pellets, pressured at 10T (see lab book pg 53)
3 samples from B3 pellets, 600MPa (see lab book pg 50)
Desired temperature = 1550C, est current = 450A
Thursday, September 28, 2017, 11:17
Vac at 8.8e-7 Torr.
Ramping TGHT up to 450A at 0.2A/min
Thursday, September 28, 2017, 17:54
Setup screen capture, see pg 53 for saved directory
Friday, September 29, 2017, 23:54
TGHT reached to 450A/7.9V, temp at 1510C.
Tapping up TGHT to 465/8.2V to reach 1550C
Pressure coming down from 1.6e-6 Torr.
See attachment 1 for the 20-hour plot
Sunday, October 01, 2017, 00:30
At around 20:00 on Sep 30, there was an increase of ~0.1 V which caused a rise in temp from 1550 to 1576C (see screen capture). Pressure increased slightly.
Tapped down TGHT to 445A/8.05V; temp maintained at 1550C.
Monday, October 02, 2017, 17:55
Cooling TGHT from 445A/8.07V, 1500oC to room temperature at 1A/min
Tuesday, October 03, 2017, 11:09
Target has been cooled for over 10 hours.
Venting chamber
|
Friday, September 15, 2017, 10:56, Laura Lambert, Ta, 42218-10, HP-SIS, Done, Conditioning Ta#54
|
Friday, September 15, 2017, 09:44
Target consists of 470 discs.
Total packed length 3.4cm [exactly 7.8cm space on both sides]
Total mass g [Incl foils + Ta wire on 6 packs]
Target consists of 350 single discs and 6x20 packs of Ta discs
Discs in target are arranged as follows: 1pack / 75singles / 1pack / 100singles / 2packs / 100singles / 1pack / 75singles / 1pack
1 long Ta Heat shield on each side, not incl center block.
No endcaps inserted, no Rh foil inserted.
Loaded into evap2 yesterday.
Chamber pumped down overnight.
TBHT will be ramped up to 230A at 1.0A/min.
TGHT will be ramped up to 650A at 2.0A/min.
Final desired temperature = 1900C
OMEGA slope = 0.98
HS water valves were already open.
Tapped up manually to 40A, vacuum stable.
IGP1 = 1.1e-6 Torr
IGP2 = 7.8e-7 Torr
Initiating auto-ramp.
Vacuum limit stop at 3.0e-5 Torr, backing off at 4.0e-5 Torr.
Monday, September 18, 2017, 08:38
TGHT = 647A, 10.04V
TBHT = 233A, 3.51V
IGP1 = 4.65e-7 Torr
IGP2 = 3.78e-7 Torr
OMEGA = 1700C
Increasing max setpoint of TGHT to 750A
Monday, September 18, 2017, 14:49
TGHT = 760A, 11.96V
TBHT = 233A, 3.54V
IGP1 = 8.9e-7 Torr
IGP2 = 8.6e-7 Torr
OMEGA = 1905C
Conditioning process complete.
Initiating auto-cool at 2.0A/min for the TGHT and 1.0A/min for the TBHT.
Tuesday, September 19, 2017, 10:38
Target was cooled down in sections so Yasser could take some temperature measurements with his thermocouples.
Vented in air and removed from evap2 this morning.
Target looks good.
Endcaps inserted and expanded.
Inserting Rh foil this afternoon.
Tuesday, September 26, 2017, 10:53
Tapped up manually to 230A over the course of ~35min.
TBHT striptool = 228A, 0.33V
TBHT direct readout = 230.4A, 0.33V
Vacuum good/ stable.
Minor spike to IGP1 = 1.5e-5 Torr ~5min after reached max setpoint of 230A.
IGP1 striptool = 3e-6 Torr
IGP1 direct readout = 3.79e-6 mBar
Initiating auto-cool at 2.0A/min.
|
Tuesday, September 12, 2017, 13:08, Aaron Schmidt, , , , , Window shutter added
|
Tuesday, September 12, 2017, 12:00:
The coated back window was changed to a shuttered window.
On star-point flange bolt interfered with the shutter, however it was removed, shortened, and re-installed.
The installation is complete. Awaiting roughing pump to leak check. |
Monday, August 21, 2017, 17:32, John Wong, SiC, , TARGET BOAT, Done, Carbonization of sol-gel SiO2+CNT
|
Monday, August 21, 2017, 17:09
Two pellets of sol-gel SiO2+CNT were produced. See lab book pg 44-46 for details.
Samples were loaded in Ta boat, wrapped with heat shield (1 layer)
Synthesis temperature = 1600C. TGHT ~ 460A/8.0V
Vacuum at 7.5 e-6 Torr.
TGHt Auto-ramp at 01A/min to reach 350A.
Thursday, August 24, 2017, 00:28
TGHT reached to 350A/5.9V, temp @ 1230C (in-line with the last measurement see elog 378).
Increase TGHT to 430, ramp at 0.1A/min.
Thursday, August 24, 2017, 23:42
TGHT reached to 430A/7.87V, temp at 1410C. Outgassing pressure reached to peak at 430A before TGHT stabilized. (Evolution of SiO(g)???)
Ramp up to 460A at 0.1A/min.
Friday, August 25, 2017, 10:30
TGHT reached to 460A/8.6V, temp at 1520C. More outgassing was observed as temp was increased.
Tapping up TGHT to reach 1600c.
Friday, August 25, 2017, 15:17
Temp reached to 1600C; TGHT at 492 A/9.3 V. Temperature was held for 3 hours. Due to a problem with the backing pump, the cooling down process was initiated.
Sample will be taken out next Monday for evaluation.
|
Tuesday, August 08, 2017, 15:00, Laura Lambert, Empty, , , Problems resolved, Wiring in PLC replaced re: IGP1 mis-communicating
|
Tuesday, August 08, 2017, 14:57
See elog i.d's #384 and #381
Investigated wiring in PLC.
Some wires in PLC were not creating a good contact - could be problem re: IGP1 tripping off.
Wires replaced by Gelo.
Pumped down and turned on power supplies over weekend.
Everything remained on - IGP1 did not trip system off.
May proceed with regular use.
|
Wednesday, August 02, 2017, 16:12, Marla Cervantes, , 40282-5, , Done, Sintering La(OH)3/C pellets
|
Monday, July 31, 2017,
Pellets previously pressed by Marla and Pauline.
Pellets are placed inside a small graphite container.
Graphite container loaded with 5 pellets was loaded into Ta-boat previously coated with TaC.
Ta-boat is wrapped with 3 Ta heat shields.
Loaded in evaporator 2.
Tuesday, August 01, 2017,
Chamber pumping down.
Wednesday, August 02, 2017, 16:03
HS water valves were opened, no leaks were detected.
Current was tapped manually to 40 A.
After the stabilization of the vacuum auto ramping was set up to 0.5 A/min.
Up to a final set up point of 300 A.
Final desired temperature ~1700 C.
|
Friday, August 04, 2017, 10:52, Laura Lambert, , 40282-5, TARGET BOAT, Problems, Sintering La(OH)3/C pellets
|
Marla Cervantes wrote: |
Monday, July 31, 2017,
Pellets previously pressed by Marla and Pauline.
Pellets are placed inside a small graphite container.
Graphite container loaded with 5 pellets was loaded into Ta-boat previously coated with TaC.
Ta-boat is wrapped with 3 Ta heat shields.
Loaded in evaporator 2.
Tuesday, August 01, 2017,
Chamber pumping down.
Wednesday, August 02, 2017, 16:03
HS water valves were opened, no leaks were detected.
Current was tapped manually to 40 A.
After the stabilization of the vacuum auto ramping was set up to 0.5 A/min.
Up to a final set up point of 300 A.
Final desired temperature ~1700 C.
|
Friday, August 04, 2017, 10:20
evap2 tripped twice yesterday.
1st trip) there was a power bump which caused a trip at ~4:20pm, this can be seen in the striptool image attached.
-TGHT spiked to zero, but immediately went back to the ~420A it was sitting at at the time.
-This did not initiate a full trip of everything, but a visual spike in the system can be seen
-Oddly this was not picked up in archives - happened so fast and must have been in the small time frame it was not picking up information
-Did TGHT actually drop to zero followed by then applying an immediate 420A?
-Or did it simple not register a reading due to power bump?
2nd trip) IGP1 stopped communicating at ~5:45pm, this can be seen in both the archives, striptool and evap2 control screenshot images attached
-IGP1 was fine, vacuum was good
-Registering good vacuum in epics - can see in screen shot vacuum was still good but IGP1 turned yellow as if turned off
-This resulted in TP followed by BV tripping off due to no longer getting a vacuum reading making the TP think there was a bad vacuum.
-Possible miscommunication with PLC?
-This is the same scenario that happened on mon - see elog i.d. 381
Will follow up when more information acquired...
|
Friday, August 04, 2017, 14:09, Laura Lambert, , 40282-5, TARGET BOAT, Done, Sintering La(OH)3/C pellets
|
Laura Lambert wrote: |
Marla Cervantes wrote: |
Monday, July 31, 2017,
Pellets previously pressed by Marla and Pauline.
Pellets are placed inside a small graphite container.
Graphite container loaded with 5 pellets was loaded into Ta-boat previously coated with TaC.
Ta-boat is wrapped with 3 Ta heat shields.
Loaded in evaporator 2.
Tuesday, August 01, 2017,
Chamber pumping down.
Wednesday, August 02, 2017, 16:03
HS water valves were opened, no leaks were detected.
Current was tapped manually to 40 A.
After the stabilization of the vacuum auto ramping was set up to 0.5 A/min.
Up to a final set up point of 300 A.
Final desired temperature ~1700 C.
|
Friday, August 04, 2017, 10:20
evap2 tripped twice yesterday.
1st trip) there was a power bump which caused a trip at ~4:20pm, this can be seen in the striptool image attached.
-TGHT spiked to zero, but immediately went back to the ~420A it was sitting at at the time.
-This did not initiate a full trip of everything, but a visual spike in the system can be seen
-Oddly this was not picked up in archives - happened so fast and must have been in the small time frame it was not picking up information
-Did TGHT actually drop to zero followed by then applying an immediate 420A?
-Or did it simple not register a reading due to power bump?
2nd trip) IGP1 stopped communicating at ~5:45pm, this can be seen in both the archives, striptool and evap2 control screenshot images attached
-IGP1 was fine, vacuum was good
-Registering good vacuum in epics - can see in screen shot vacuum was still good but IGP1 turned yellow as if turned off
-This resulted in TP followed by BV tripping off due to no longer getting a vacuum reading making the TP think there was a bad vacuum.
-Possible miscommunication with PLC?
-This is the same scenario that happened on mon - see elog i.d. 381
Will follow up when more information acquired...
|
Friday, August 04, 2017, 14:05
Vented in air and transferred to glove box today.
Container did not break.
Some wires in PLC were not creating a good contact - could be problem re: IGP1 tripping off.
Wires replaced by Gelo.
Put back under vacuum with nothing loaded over weekend to see how things run...
|
Tuesday, August 01, 2017, 15:34, Laura Lambert, , , , Problems, IGP1 mis-communicating with EPICS - PLC problem?
|
Monday, July 31, 2017, 15:24
Turned on BV and TP this afternoon.
Started ramping down, ~1min after turned on both tripped off.
Vacuum box turned red.
IGP1 appears yellow but still registering a vacuum.
TP interlocks: requires IEVAP2:IGP1 < 500mTorr but IGP1 = 6mTorr when tripped off.
Should have been satisfied and therefore not tripped but IGP1 not communicating?
Nothing wrong with ion gauge in person, vacuum good on direct read out.
When attempting 'Global Reset', nothing would reset - vacuum box remained red etc.
See screenshot attached of errors.
Tuesday, August 01, 2017, 15:31
Had kept BP, PV and RV overnight.
This morning vacuum fine, everything had reset except "IEVAP2:TP on" under device notes for IEVAP2:TP remained red.
Turned on BV and TP, once turbo pump registered on, red wording went away.
Currently pumping down - everything looks fine now.
Still unsure of reason for these errors...
Friday, August 04, 2017, 10:55
Happened again last night at ~5:45 while evaps at ~420A - see elog i.d. 383 for photos and details.
|
Wednesday, July 19, 2017, 13:55, Marla Cervantes, , 40282-5, TARGET BOAT, Done, Sintering La(OH)3/C discs
|
Wednesday, July 19, 2017, 13:44
Discs previously casted by Marla and Pauline and weighed.
Discs are placed inside a small graphite container.
Graphite container with discs loaded with 30 discs was loaded into Ta-boat previously coated with TaC.
Ta-boat is wrapped with 3 Ta heat shields.
Loaded in evaporator 2.
Chamber currently pumping down.
Thursday, July 20, 2017, 16:07
HS water valves were opened in the morning, no leaks were detected.
Perform water test to confirm paddle wheels are working well.
Current was tapped manually to 40 A.
Read out on meter confirmed paddle wheels are registering
Tap back down to 20 A, tripped off system on purpose by closing HS water valves.
TGHT tripped off as expected.
Water flow test was good, initiating ramp up of samples.
Taped manually to 40 A.
After the stabilization of the vacuum auto ramping was set up to 0.2 A/min.
Up to a final set up point of 250 A.
Final desired temperature ~1800 C.
Friday, July 21, 2017, 10:20
Final set up from July 20 was reached.
Current reading: 244.6 A.
Voltage reading: 3.82 V.
Temperature reached: 1105 C.
Final set up was change to 1500 A.
The temperature reached at 6 pm was 1936 C so the current was decreased to 488 A.
The final temperature after 30 min was 1800 C.
The set up stayed the same for the weekend.
Monday, July 24, 2017, 13:06
Temperature reading in the morning was 1856 C.
TGHT: 487.87 A, 9.07 V
TGHT power supply:
IGP1: 3.75e-7 Torr
IGP2: 3.51e-7 Torr
Started to ramp down at 1 A/min rate.
Initiating auto cooling at 1.0A/min for TGHT.
Tuesday, July 25, 2017, 09:27
LaC2/C discs were taken off of evap2.
LaC2/C discs were brought in to glove box.
|
Tuesday, July 18, 2017, 15:30, Laura Lambert, , , , Maintenance, Paddle wheel replacement for all evap2 water supplies
|
Tuesday, July 18, 2017, 15:26
Problems occured with TGHT water supply paddle wheel stopped and therefore tripped off evap2 last week.
All paddle wheels were replaced today for evap2 [other than the chiller].
A build up of dirt was found on all wheels replaced.
Evap2 good to go.
Will test flow meters before heating up to higher setpoints to confirm everything is working.
|
Monday, July 10, 2017, 17:36, John Wong, np-SiC, , TARGET BOAT, Problems, Water Sensor Problem, TGHT Tripped. (np-SiC fibrous Pellet: Applied pressure vs Density)
|
Monday, July 10, 2017, 17:28
Two np-SiC fibrous pellets with different applied pressure:
1) 200MPa, 2) 335 MPa (see logbook pg 36 for more details).
Desired heating temperature: 1550C (Previous setting: TGHT 400A/6.94V)
Two layers of Ta foils wrapped around the target boat.
Chamber is pumping down...
Tuesday, July 11, 2017, 11:11
Pressured came down to 1.0e-6 Torr.
Tapping up TGHT.
Tuesday, July 11, 2017, 11:24
Tapped TGHT up to 45A - pressure stabilized at around 3.0e-5 Torr.
Auto ramp 1.0A/min to reach 350A before tapping up further.
Wednesday, July 12, 2017, 10:59
TGHT reached to 350A/5.5V, temp @ 1270C - much lower than expected; could be a short between the target container and the heat shield. I actually had a had time adjusting the target legs to avoid shorting the cu-heat shield.
Tapped TGHT further up to 375A/6.07V, Omega Temp at 1340C. Holding current for about 50 mins, re-measured with pyrometer - temperature matches.
Wednesday, July 12, 2017, 14:49
TGHT set at 450A/7.7A. Temp at ~1550C. See attachment for temp plot
Holding at temp for 5 days before cooling down on Monday July 17.
Thursday, July 13, 2017, 17:52
TGHT tripped off due to bad IEVAP2:WFB1 water flow. Not sure what was the cause. Will leave the heater off for now and investigate this tomorrow.
Friday, July 14, 2017, 11:48
Investigated the bad water flow situation. It was due to a faulty water flow sensor. The paddle wheel stopped turning until I gave it a tab. We had a similar problem before with the water sensor, see elog ID 109. It is probably the time to replace all the water sensors.
|
Tuesday, June 20, 2017, 16:07, Laura Lambert, Ta, 42218-6, HP-SIS, Done, Conditioning Ta#53
|
Tuesday, June 20, 2017, 15:58
Target consists of 470 discs.
Total packed length 3.4cm [exactly 7.8cm space on both sides]
Total mass 50.3105g [Incl foils + Ta wire on 6 packs]
Target consists of 350 single discs and 6x20 packs of Ta discs
Discs in target are arranged as follows: 1pack / 75singles / 1pack / 100singles / 2packs / 100singles / 1pack / 75singles / 1pack
1 long Ta Heat shield.
No endcaps inserted, no Rh foil inserted.
Chamber currently pumping down.
TBHT will be ramped up to 230A at 1.0A/min.
TGHT will be ramped up to 600A at 2.0A/min.
Final desired temperature = 1900C
OMEGA slope = 0.98
Vacuum limit stop at 3.0e-5 Torr, backing off at 4.0e-5 Torr.
*Note: container accidentally engraved with WO#412218-6 when it should be WO#42218-6
Wednesday, June 21, 2017, 10:05
HS water valves opened, no leaks detected.
Tapped up manually to 40A, vacuum stable.
IGP1 = 5.53e-7 Torr
IGP2 = 4.35e-7 Torr
Initiating auto-ramp.
Wednesday, June 21, 2017, 14:48
TGHT stopped at 575A due to voltage limit sitting at 9V
Increased max setpoint of voltage to 14V.
Re-started auto-ramp starting at 575A.
Wednesday, June 21, 2017, 15:23
TGHT = 600A, 8.95V
TBHT = 230A, 3.72V
IGP1 = 1.55e-6 Torr
IGP2 = 1.62e-6 Torr
OMEGA = 1538C
Increasing max setpoint of TGHT to 700A
Wednesday, June 21, 2017, 16:21
TGHT = 700A, 10.57V
TBHT = 230A, 3.75V
IGP1 = 2.2e-6 Torr
IGP2 = 2.4e-6 Torr
OMEGA = 1730C
Increasing max setpoint of TGHT to 750A
Friday, June 23, 2017, 15:41
TGHT = 780A, 11.77V
TBHT = 230A, 3.77V
IGP1 = 4.8e-7 Torr
IGP2 = 4.8e-7 Torr
OMEGA = 1890C
Conditioning process complete.
Initiating auto-cool at 2.0A/min for the TGHT and 1.0A/min for the TBHT.
Monday, June 26, 2017, 10:51
Target vented in air and removed from evap2 today.
Endcaps inserted.
Target looks good!
|
Wednesday, June 14, 2017, 15:51, Laura Lambert, SiC, 40282-4, TARGET BOAT, In progress, Sintering SiC pellets
|
Wednesday, June 14, 2017, 15:49
Pellets previously made by Marla and weighed.
Pellets are placed inside a small graphite sample tube.
Graphite sample tube loaded with pellets is loaded into a previously TaC coated boat.
Boat is wrapped with 3x Ta heat shields.
Loaded into evap2.
Chamber currently pumping down.
Thursday, June 15, 2017, 11:24
HS water valves were opened this morning, no leaks detected.
Tapped up manually to 50A, 0.44V
Vacuum currently rising starting to settle.
IGP1 = 1.51e-6 Torr.
One vacuum stabilizes will initiate auto ramp at a rate of 1.0 A/min up to a final set point of 150 A.
Final desired temperature of 1800C.
|
Friday, June 16, 2017, 10:42, Marla Cervantes, SiC, 40282-4, TARGET BOAT, Done, Sintering SiC pellets
|
Laura Lambert wrote: |
Wednesday, June 14, 2017, 15:49
Pellets previously made by Marla and weighed.
Pellets are placed inside a small graphite sample tube.
Graphite sample tube loaded with pellets is loaded into a previously TaC coated boat.
Boat is wrapped with 3x Ta heat shields.
Loaded into evap2.
Chamber currently pumping down.
Thursday, June 15, 2017, 11:24
HS water valves were opened this morning, no leaks detected.
Tapped up manually to 50A, 0.44V
Vacuum currently rising starting to settle.
IGP1 = 1.51e-6 Torr.
One vacuum stabilizes will initiate auto ramp at a rate of 1.0 A/min up to a final set point of 150 A.
Final desired temperature of 1800C.
|
Friday, June 16, 2017, 10:37
IGP1 = 7.91e-7 torr.
TGHT = 167 A, 2.3 V.
Tapped up manually to 350A yesterday, remained there overnight.
IGP1 = 4.55e-7 torr
TGHT=350 A, 5.6 V,
Changed slope to 0.98
Checked temperature readings with mikron to confirm slope
Mikron LS = 1260C, RS=1290C
OMEGA= 1295C
Initiating auto ramp at 1.0A/min to a final set point of 450A.
Final desired temperature of 1600C (no longer need to go to 1800C).
*note: graphite sample tube has graphite endcaps inserted
|
Friday, June 16, 2017, 15:14, Laura Lambert, SiC, 40282-4, TARGET BOAT, Done, Sintering SiC pellets
|
Marla Cervantes wrote: |
Laura Lambert wrote: |
Wednesday, June 14, 2017, 15:49
Pellets previously made by Marla and weighed.
Pellets are placed inside a small graphite sample tube.
Graphite sample tube loaded with pellets is loaded into a previously TaC coated boat.
Boat is wrapped with 3x Ta heat shields.
Loaded into evap2.
Chamber currently pumping down.
Thursday, June 15, 2017, 11:24
HS water valves were opened this morning, no leaks detected.
Tapped up manually to 50A, 0.44V
Vacuum currently rising starting to settle.
IGP1 = 1.51e-6 Torr.
One vacuum stabilizes will initiate auto ramp at a rate of 1.0 A/min up to a final set point of 150 A.
Final desired temperature of 1800C.
|
Friday, June 16, 2017, 10:37
IGP1 = 7.91e-7 torr.
TGHT = 167 A, 2.3 V.
Tapped up manually to 350A yesterday, remained there overnight.
IGP1 = 4.55e-7 torr
TGHT=350 A, 5.6 V,
Changed slope to 0.98
Checked temperature readings with mikron to confirm slope
Mikron LS = 1260C, RS=1290C
OMEGA= 1295C
Initiating auto ramp at 1.0A/min to a final set point of 450A.
Final desired temperature of 1600C (no longer need to go to 1800C).
*note: graphite sample tube has graphite endcaps inserted
|
Friday, June 16, 2017, 15:10
Tapped up manually to 420A and auto ramp at 1.0A/min to 450A.
IGP1= 7.15e-7 torr
TGHT=450 A, 7.85 V
OMEGA = 1605C
Process completed, initiating auto cool at 1.0A/min
Elog entry by Pauline
Monday, June 19, 2017, 16:18
Vented in air and removed from evap2 this a.m.
Weirdly TGHT had tripped off at 10pm on friday June 16th
TGHT = 58A when it tripped off.
Nothing else tripped.
Power supply was still on.
Water was still running
But, in the epics water control box it showed green boxes for TGHT, HS and CHILLER...but all said trip in yellow next to the boxes...odd...
Also noted, before removing from evap2, noticed both legs were bent and touching heat shield, will look further into this...
|
Monday, June 05, 2017, 15:20, Laura Lambert, Empty, 42218-15, LP-SIS, Done, Sintering TaC coating on UCx#21 container
|
Monday, June 05, 2017, 15:20
Container coated with TaC using 'flushing technique' and let dry over weekend.
Cleaned ionizer tube with acetone, no coating inside ionizer tube.
Wrapped with 3 x Ta heat shields, incl center block
Currently pumping down in evap2
OMEGA slope = 0.98
Good vac at 3.0e-5, bad vac at 4.0e-5 Torr.
Tuesday, June 06, 2017, 10:00
First time not turning water off and flushing lines after last use.
HS water valves have remained open since the last time evap2 was used [conditioning Ta#52]
No leak check done.
Tapped up manually to 35A.
Waited ~25min
Vacuum stable.
IGP1 = 2.9e-6 Torr
IGP2 = 4.8e-6 Torr
Initiating auto ramp for TGHT @ 0.2A/min to a max setpoint of 350A
Initiating auto ramp for TBHT @ 0.1A/min to a max setpoint of 230A
Once max setpoints achieved, will tap up manually to final desired temperature of 1900C
Wednesday, June 07, 2017, 09:26
TGHT = 304A, 4.46V
TBHT = 169A, 2.769V
IGP1 = 6.1e-7 Torr
IGP2 = 7.3e-7 Torr
Vacuum stable.
Increasing ramping rate to 1.0A/min and 0.5A/min for the TGHT and TBHT respectively.
Wednesday, June 07, 2017, 10:40
TGHT = 350A, 5.28V
TBHT = 203A, 3.39V
IGP1 = 1e-6 Torr
Increasing ramping rate for TBHT to 1.0A/min
Wednesday, June 07, 2017, 12:10
TGHT = 350A, 5.26V
TBHT = 230A, 3.99V
IGP1 = 7.0e-7 Torr
IGP2 = 8.3e-7 Torr
OMEGA = 1600C
Vacuum stable.
Increasing max setpoint of TGHT to 400A
Re-initiating ramping rate of TGHT at 1.0A/min
Wednesday, June 07, 2017, 15:42
Tapped up to reach final desired temperature.
TGHT = 450A, 7.28V
TBHT = 230A, 4.02V
IGP1 = 9.0e-7 Torr
IGP2 = 1.07e-6 Torr
OMEGA = 1910C
Will remain at max setpoints overnight.
Thursday, June 08, 2017, 08:51
Remained at max setpoints for 17hrs.
TGHT = 450A, 7.28V
TBHT = 230A, 4.02V
IGP1 = 2.6e-7 Torr
IGP2 = 2.9e-7 Torr
OMEGA = 1899C
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Thursday, June 08, 2017, 16:28
Vented in air and taken out this afternoon.
Container looks good!
Transferred into glove box.
|
Tuesday, May 30, 2017, 14:40, Laura Lambert, Ta, 42218-14, LP-SIS, Done, Conditioning Ta#52
|
Tuesday, May 30, 2017, 14:36
Target consists of 400 discs.
Total packed length 2.9cm [exactly 8.05cm space on both sides]
Total mass 42.8228g [Incl foils + Ta wire on 4 packs]
Target consists of 320 single discs and 4x20 packs of Ta discs
Discs in target are arranged as follows: 80singles / 1pack / 80singles / 2packs / 80singles / 1pack / 80singles
3x Ta Heat shields.
No endcaps inserted, no Rh foil inserted.
Chamber currently pumping down.
TBHT will be ramped up to 230A at 1.0A/min.
TGHT will be ramped up to 350A at 2.0A/min.
Final desired temperature = 1900C
OMEGA slope = 0.98
Windows cleaned.
Vacuum limit stop at 3.0e-5 Torr, backing off at 4.0e-5 Torr.
Wednesday, May 31, 2017, 09:47
HS water valves opened, no leaks detected.
Tapped up manually to 35A.
Vacuum stable.
IGP1 = 4.58e-7 Torr
IGP2 = 3.68e-7 Torr
Initiating auto ramp.
Wednesday, May 31, 2017, 14:07
IGP1 = 1.11e-6 Torr
IGP2 = 1.13e-6 Torr
TGHT = 354A, 5.45V
TBHT =233A, 4.01V
OMEGA = 1565C
Increasing max setpoint to 400A at same ramping rate.
Wednesday, May 31, 2017, 14:41
IGP1 = 1.19e-6 Torr
IGP2 = 1.24e-6 Torr
TGHT = 401A, 6.37V
OMEGA = 1708C
Increasing max setpoint to 425A at same ramping rate.
Wednesday, May 31, 2017, 15:51
Tapped up to ~1900C
TGHT = 480A, 7.85V
TBHT = 230A, 4.06V
OMEGA = 1912C
IGP1 = 1.85e-6 Torr
IGP2 = 2.06e-6 Torr
Will remain at max setpoints for a couple days before cooling
Friday, June 02, 2017, 13:19
Remained at max setpoint for 2days
TGHT = 480A, 7.85V
TBHT = 230A, 4.06V
OMEGA = 1885C
IGP1 = 2.15e-7 Torr
IGP2 = 2.07e-7 Torr
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Monday, June 05, 2017, 15:18
Vented in air and taken out this morning.
Target looks good
Wednesday, June 07, 2017, 15:41
Endcaps inserted.
Ta heat shield removed.
Rh foil inserted.
Handed off to assembly.
|
Tuesday, May 16, 2017, 11:57, Laura Lambert, SiC, 41369-10, HP-FEBIAD-CTL, Done, Sintering SiC#36
|
Tuesday, May 16, 2017, 10:56
Target container contains 460 discs of SiC
Target packed length = 17cm.
Mass of SiC(green) = 55.5152g
Consists of 4 packs of 5 and 440 singles.
Container is wrapped with 1x heatshield around each side of cooling fins; no end caps are inserted yet - coated spring inserted both sides to hold discs in place.
Sintering temp = 1800C
Chamber is currently being pumped down.
Tuesday, May 16, 2017, 15:27
HS water valves turned on, no leaks detected.
Tapped up manually to 30A
Waited ~30min , vacuum stable.
IGP1 = 8.25e-6 Torr
Initiating auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
TGHT max = 400A. TBHT max at 230A.
Slope on OMEGA = 1.09 [see elog i.d. # 370 for reasoning behind OMEGA slope choice]
Friday, May 19, 2017, 10:13
TGHT = 250A, 3.11V DR = 248A, 3.3V
TBHT = 137A, 1.68V DR = 140A, 1.73V
OMEGA = 1100C
IGP1= 6.9e-6 Torr DR = 1e-5mbar
IGP2 = 5.9e-6 Torr DR = 6.45e-6 Torr
Vacuum stable.
Increasing ramping rate to 1.0A/min and 0.5A/min for the TGHT and TBHT respectively.
Friday, May 19, 2017, 10:33
Change in plan and switching ramping rate to 0.5A/min and 0.2A/min for the TBHT and TGHT respectively.
Friday, May 19, 2017, 14:49
TGHT = 400A, 5.46
TBHT = 200A, 2.66
IGP1 = 2.7e-5 Torr
IGP2 = 2.2e-5 Torr
OMEGA = 1200C
Increasing max setpoint for TGHT to 550A
Decreasing ramping rate to 0.2A/min and 0.1A/min for over the weekend.
Tuesday, May 23, 2017, 09:23
TGHT = 550A, 8.37
TBHT = 230A, 3.14
IGP1 = 1.6e-7 Torr
IGP2 = 1.6e-7 Torr
OMEGA = 1570C
Increasing max setpoint for TGHT to 600A at rate to 0.5A/min
Tuesday, May 23, 2017, 11:45
TGHT = 600A, 9.36
IGP1 = 3.5e-7 Torr
IGP2 = 3.8e-7 Torr
OMEGA = 1675C
Increasing max setpoint for TGHT to 625A at rate to 0.5A/min
Tuesday, May 23, 2017, 13:03
TGHT = 625A, 9.80V
IGP1 = 5.2e-7 Torr
IGP2 = 5.7e-7 Torr
OMEGA = 1715C
OMEGA no longer valid around 640A as temperature drops instantly after tapping up.
Could be due to target movement at high temperature.
No obvious window coating.
Tapped up manually to 660A, 10.49V.
Will remain at max setpoint overnight.
Wednesday, May 24, 2017, 11:13
TGHT = 660A, 10.74V
TGHT power supply = 662A, 11.00V
TBHT = 230A, 3.16V
TBHT power supply = 232A, 3.25V
IGP1 = 4.2e-7 Torr
IGP1 direct readout = 5.9e-7 mbar
IGP2 = 4.6e-8 Torr
IGP2 direct readout = 5e-7 Torr
Evap2 reached max setpoint yesterday afternoon.
Window has thiny coating - see attached photo.
OMEGA = 1800
MIKRON = ~1800
Initiating auto cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Wednesday, May 24, 2017, 11:36
Change of plan.
TGHT = 620A, TBHT = 210A
Ramping back-up to max setpoints and will remain at those points until vacuum starts to decrease more.
Friday, May 26, 2017, 15:24
IGP1 = 2.1e-7 Torr
IGP2 = 2.2e-7 Torr
TGHT = 660A, 10.72V
TBHT = 230A, 3.21V
All windows coated.
Remained at max setpoints for ~3.5days.
Conditioning process complete.
Initiating auto-cool at 2A/min and 1A/min for the TGHT and TBHT respectively.
Tuesday, May 30, 2017, 14:41
Target vented in air and removed from evap2
Looks good!
Endcaps inserted and expanded.
See photos attached.
|
Thursday, April 27, 2017, 15:54, Laura Lambert, SiC, 39530-10, HP-FEBIAD, In progress, Sintering SiC#36
|
Thursday, April 27, 2017, 14:01
Target container contains 470 discs of SiC
Target packed length = 16cm.
Mass of SiC(green) = 52.13g
Discs in target are arranged as follows: 5singles / 1pack / 65singles / 1pack / 75singles / 1pack / 75singles / 2packs / 75singles / 1pack / 75singles / 1pack / 55singles / 1pack / 5singles
Container is wrapped with 1x heatshield around each side of cooling fins; no end caps are inserted yet - coated spring inserted both sides to hold discs in place.
Sintering temp = 1800C
Chamber is currently being pumped down.
Friday, April 28, 2017, 13:06
HS water valves turned on this morning, no leaks detected.
Tapped up manually to 40A
Waited ~3hrs , vacuum stable.
IGP1 = 4.13e-6 Torr
Initiating auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
TGHT max = 400A. TBHT max at 230A.
Slope on OMEGA = 1.08 [see elog i.d. # 326 for reasoning behind OMEGA slope choice]
Tuesday, May 02, 2017, 09:24
IGP1 = 2.34e-6 Torr
TBHT = 230A, 3.15V
TGHT = 298A, 3.96V
OMEGA = 1030C
Vacuum stable, increasing ramping rate up to 0.5A/min
Tuesday, May 02, 2017, 13:20
IGP1 = 1.3e-5 Torr
TGHT = 400A, 5.6V
OMEGA = 1175C
Increasing max setpoint to 500A
|
Wednesday, May 03, 2017, 13:48, Laura Lambert, SiC, 39530-10, HP-FEBIAD, Problems, Sintering SiC#36
|
Laura Lambert wrote: |
Thursday, April 27, 2017, 14:01
Target container contains 470 discs of SiC
Target packed length = 16cm.
Mass of SiC(green) = 52.13g
Discs in target are arranged as follows: 5singles / 1pack / 65singles / 1pack / 75singles / 1pack / 75singles / 2packs / 75singles / 1pack / 75singles / 1pack / 55singles / 1pack / 5singles
Container is wrapped with 1x heatshield around each side of cooling fins; no end caps are inserted yet - coated spring inserted both sides to hold discs in place.
Sintering temp = 1800C
Chamber is currently being pumped down.
Friday, April 28, 2017, 13:06
HS water valves turned on this morning, no leaks detected.
Tapped up manually to 40A
Waited ~3hrs , vacuum stable.
IGP1 = 4.13e-6 Torr
Initiating auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
TGHT max = 400A. TBHT max at 230A.
Slope on OMEGA = 1.08 [see elog i.d. # 326 for reasoning behind OMEGA slope choice]
Tuesday, May 02, 2017, 09:24
IGP1 = 2.34e-6 Torr
TBHT = 230A, 3.15V
TGHT = 298A, 3.96V
OMEGA = 1030C
Vacuum stable, increasing ramping rate up to 0.5A/min
Tuesday, May 02, 2017, 13:20
IGP1 = 1.3e-5 Torr
TGHT = 400A, 5.6V
OMEGA = 1175C
Increasing max setpoint to 500A
|
Wednesday, May 03, 2017, 13:33
TGHT had remained at 500A for 16hrs, vacuum had initially come down nicely.
Vacuum was starting to creep up when i came in this morning before 8am, IGP1 was at 1.2e-5 Torr
TGHT = 500A, 7.77V
OMEGA = 1440C
Around 8:30 vacuum started to spike, so the TGHT was tapped down rapidly to 450A
Tapping the TGHT down made no difference to the vacuum.
By the time 450A was hit, it was too late and the spike in vacuum caused the evaporator to trip off.
Turbo pump in epics showed on, turbo pump showed on according to TP direct controls.
Everything was shut off and the venting tapped, this made it obvious the turbo pump was already off as there was no ramping down noises from the turbo pump.
TP control box turned off then on again, at this point the controls showed a 'fail' message.
Turns out the turbo pump control box was fried and that's what had caused the turbo pump to fail with no notice in epics causing the vacuum to spontaneously spike.
Waiting on a new one from vacuum group...
See photos attached of striptool screenshots.
Wednesday, May 03, 2017, 15:03
New TP control boxed installed.
Turbo pump turned on, everything pumped down.
Vacuum good, IGP1 = 6.92e-7 Torr.
IGP2 still not working, won't turn on via epics.
Tried unplugging and plugging back in...still appears red with 'fail' message...
|
Wednesday, May 03, 2017, 16:09, Laura Lambert, SiC, 39530-10, HP-FEBIAD, Problems resolved, Sintering SiC#36
|
Laura Lambert wrote: |
Laura Lambert wrote: |
Thursday, April 27, 2017, 14:01
Target container contains 470 discs of SiC
Target packed length = 16cm.
Mass of SiC(green) = 52.13g
Discs in target are arranged as follows: 5singles / 1pack / 65singles / 1pack / 75singles / 1pack / 75singles / 2packs / 75singles / 1pack / 75singles / 1pack / 55singles / 1pack / 5singles
Container is wrapped with 1x heatshield around each side of cooling fins; no end caps are inserted yet - coated spring inserted both sides to hold discs in place.
Sintering temp = 1800C
Chamber is currently being pumped down.
Friday, April 28, 2017, 13:06
HS water valves turned on this morning, no leaks detected.
Tapped up manually to 40A
Waited ~3hrs , vacuum stable.
IGP1 = 4.13e-6 Torr
Initiating auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
TGHT max = 400A. TBHT max at 230A.
Slope on OMEGA = 1.08 [see elog i.d. # 326 for reasoning behind OMEGA slope choice]
Tuesday, May 02, 2017, 09:24
IGP1 = 2.34e-6 Torr
TBHT = 230A, 3.15V
TGHT = 298A, 3.96V
OMEGA = 1030C
Vacuum stable, increasing ramping rate up to 0.5A/min
Tuesday, May 02, 2017, 13:20
IGP1 = 1.3e-5 Torr
TGHT = 400A, 5.6V
OMEGA = 1175C
Increasing max setpoint to 500A
|
Wednesday, May 03, 2017, 13:33
TGHT had remained at 500A for 16hrs, vacuum had initially come down nicely.
Vacuum was starting to creep up when i came in this morning before 8am, IGP1 was at 1.2e-5 Torr
TGHT = 500A, 7.77V
OMEGA = 1440C
Around 8:30 vacuum started to spike, so the TGHT was tapped down rapidly to 450A
Tapping the TGHT down made no difference to the vacuum.
By the time 450A was hit, it was too late and the spike in vacuum caused the evaporator to trip off.
Turbo pump in epics showed on, turbo pump showed on according to TP direct controls.
Everything was shut off and the venting tapped, this made it obvious the turbo pump was already off as there was no ramping down noises from the turbo pump.
TP control box turned off then on again, at this point the controls showed a 'fail' message.
Turns out the turbo pump control box was fried and that's what had caused the turbo pump to fail with no notice in epics causing the vacuum to spontaneously spike.
Waiting on a new one from vacuum group...
See photos attached of striptool screenshots.
Wednesday, May 03, 2017, 15:03
New TP control boxed installed.
Turbo pump turned on, everything pumped down.
Vacuum good, IGP1 = 6.92e-7 Torr.
IGP2 still not working, won't turn on via epics.
Tried unplugging and plugging back in...still appears red with 'fail' message...
|
Wednesday, May 03, 2017, 16:07
Unplugging and plugging back in seemed to work now that evap2 under vacuum
IGP2 works again.
Will look into replacement ion gauge...
|
Wednesday, May 03, 2017, 16:10, Laura Lambert, SiC, 39530-10, HP-FEBIAD, Done, Sintering SiC#36 8x
|
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Thursday, April 27, 2017, 14:01
Target container contains 470 discs of SiC
Target packed length = 16cm.
Mass of SiC(green) = 52.13g
Discs in target are arranged as follows: 5singles / 1pack / 65singles / 1pack / 75singles / 1pack / 75singles / 2packs / 75singles / 1pack / 75singles / 1pack / 55singles / 1pack / 5singles
Container is wrapped with 1x heatshield around each side of cooling fins; no end caps are inserted yet - coated spring inserted both sides to hold discs in place.
Sintering temp = 1800C
Chamber is currently being pumped down.
Friday, April 28, 2017, 13:06
HS water valves turned on this morning, no leaks detected.
Tapped up manually to 40A
Waited ~3hrs , vacuum stable.
IGP1 = 4.13e-6 Torr
Initiating auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
TGHT max = 400A. TBHT max at 230A.
Slope on OMEGA = 1.08 [see elog i.d. # 326 for reasoning behind OMEGA slope choice]
Tuesday, May 02, 2017, 09:24
IGP1 = 2.34e-6 Torr
TBHT = 230A, 3.15V
TGHT = 298A, 3.96V
OMEGA = 1030C
Vacuum stable, increasing ramping rate up to 0.5A/min
Tuesday, May 02, 2017, 13:20
IGP1 = 1.3e-5 Torr
TGHT = 400A, 5.6V
OMEGA = 1175C
Increasing max setpoint to 500A
|
Wednesday, May 03, 2017, 13:33
TGHT had remained at 500A for 16hrs, vacuum had initially come down nicely.
Vacuum was starting to creep up when i came in this morning before 8am, IGP1 was at 1.2e-5 Torr
TGHT = 500A, 7.77V
OMEGA = 1440C
Around 8:30 vacuum started to spike, so the TGHT was tapped down rapidly to 450A
Tapping the TGHT down made no difference to the vacuum.
By the time 450A was hit, it was too late and the spike in vacuum caused the evaporator to trip off.
Turbo pump in epics showed on, turbo pump showed on according to TP direct controls.
Everything was shut off and the venting tapped, this made it obvious the turbo pump was already off as there was no ramping down noises from the turbo pump.
TP control box turned off then on again, at this point the controls showed a 'fail' message.
Turns out the turbo pump control box was fried and that's what had caused the turbo pump to fail with no notice in epics causing the vacuum to spontaneously spike.
Waiting on a new one from vacuum group...
See photos attached of striptool screenshots.
Wednesday, May 03, 2017, 15:03
New TP control boxed installed.
Turbo pump turned on, everything pumped down.
Vacuum good, IGP1 = 6.92e-7 Torr.
IGP2 still not working, won't turn on via epics.
Tried unplugging and plugging back in...still appears red with 'fail' message...
|
Wednesday, May 03, 2017, 16:07
Unplugging and plugging back in seemed to work now that evap2 under vacuum
IGP2 works again.
Will look into replacement ion gauge...
|
Wednesday, May 03, 2017, 16:09
HS water valves opened, no leaks detected.
Tapped up manually to 40A.
Vacuum stable.
IGP1 = 3.6e-7 Torr
Initiated auto-ramp at 1.0A/min and 0.5A/min to 300A and 230A for the TGHT and TBHT respectively.
Thursday, May 04, 2017, 08:41
Reached 300A, 230A 10hrs ago.
IGP1 = 1.5e-7 Torr
OMEGA = 1070C
Increasing max setpoint to 500A at a rate of 0.5A/min for TGHT
Thursday, May 04, 2017, 14:58
Back up to max setpoint that was reached before evap2 tripped off.
TGHT = 500A, 7.65V
IGP1 = 9.3e-7 Torr
OMEGA = 1450C
Increasing max setpoint to 550A, ramping up at a lower rate of 0.2A/min since this will be done overnight.
Friday, May 05, 2017, 08:53
TGHT = 550A, 8.64V
IGP1 = 2.8e-7 Torr
OMEGA = 1560C
Increasing max setpoint to 600A at a ramping rate of 0.5A/min
Friday, May 05, 2017, 11:09
TGHT = 600A, 9.58V
IGP1 = 7.3e-7 Torr
OMEGA = 1670C
Increasing max setpoint to 625A at a ramping rate of 0.5A/min
Friday, May 05, 2017, 12:05
TGHT = 625A, 10.05V
IGP1 = 9.9e-7 Torr
OMEGA = 1710C
Increasing max setpoint to 650A at a ramping rate of 0.5A/min
Friday, May 05, 2017, 13:13
TGHT = 650A, 10.57V
IGP1 = 1.1e-6 Torr
OMEGA = 1740C
Mikron through left side windown on outside bottom left edge on container = 1750C
Tapping up manually to 1800C
Friday, May 05, 2017, 13:42
Adjusted slope to 1.09 so same spot on leg using MIKRON = OMEGA
TGHT = 680A, 11.08V
IGP1 = 1.6e-6 Torr
OMEGA = 1795C
MIKRON = 1795C
Plotting a temperature curve, the predicted required current to reach 1800C was 670A using a slope of 1.08
Currently sitting 10A above predicted required current.
After several minutes, temperature dropped a few degrees to 1790C
Window remains clear and uncoated.
Tapped up to TGHT = 685A, 11.2V
OMEGA = 1795C
Will remain at this setpoint over the weekend.
Monday, May 08, 2017, 08:59
TGHT = 685A, 11.08V
TBHT = 230A, 3.24V
IGP1 = 1.98e-7 Torr
OMEGA has lowered to 1342C
Evap2 sat at max setpoints over the wknd.
Will check window port before cooling...
*UPDATE ON TRIP-OFF*
A closer look into the details using archives [see photos attached]:
TP tripped off TBHT and TGHT at ~8e-5Torr
Anything in the evaporator requires ~1hr to cool before turning things off.
In this scenario, the target was @ ~1440C. so ~30min post TP trip, the target may still be at ~1000C.
Anything above 0.02Torr could be close enough to atmopheric pressure that this would be cooling too fast and could lead to breaking the target/ cracking the Ta metal.
As one can see in the screenshots attached, the vacuum lingered around 0.005Torr for ~2hrs before anything was done.
This provided enough time for the target to cool before it was introduced to atmospheric pressure when the BV was closed when trying to figure out the problem.
In summary, the target 'should' be OK...will inspect target further when removed from the evaporator.
Tuesday, May 09, 2017, 09:16
TGHT = 685A, 11.04V
TGHT power supply = 686A, 11.31V
TBHT = 230A, 3.24V
TBHT power supply = 236A, 3.32V
IGP1 = 1.6e-7 Torr
IGP1 direct readout = 2.3e-7 mbar
IGP2 = 6.8e-8 Torr
IGP2 direct readout = 8.46e-8 Torr
Evap2 reached max setpoint friday afternoon.
Window clearly coated - see attached photo.
Initiating auto cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Wednesday, May 10, 2017, 09:18
Vented in air and opened up this morning.
Inspected container carefully for any cracks/ marks due to TP tripping off at 1450C
Target looks good!
One sample disc removed for SEM.
When removing disc for sample, the SiC came off the graphite backing and just SiC flake came out - see photo
Photos attached showing inside container with no Si crystal formation/ good clear path all the way through target and sample removed for tests
|
Thursday, May 11, 2017, 11:36, Laura Lambert, SiC, 39530-10, HP-FEBIAD, Done, Sintering SiC#36 - not SiC#36: now back-up [SiC#36 should be HP-FEBIAD-CTL!!!]
|
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Thursday, April 27, 2017, 14:01
Target container contains 470 discs of SiC
Target packed length = 16cm.
Mass of SiC(green) = 52.13g
Discs in target are arranged as follows: 5singles / 1pack / 65singles / 1pack / 75singles / 1pack / 75singles / 2packs / 75singles / 1pack / 75singles / 1pack / 55singles / 1pack / 5singles
Container is wrapped with 1x heatshield around each side of cooling fins; no end caps are inserted yet - coated spring inserted both sides to hold discs in place.
Sintering temp = 1800C
Chamber is currently being pumped down.
Friday, April 28, 2017, 13:06
HS water valves turned on this morning, no leaks detected.
Tapped up manually to 40A
Waited ~3hrs , vacuum stable.
IGP1 = 4.13e-6 Torr
Initiating auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
TGHT max = 400A. TBHT max at 230A.
Slope on OMEGA = 1.08 [see elog i.d. # 326 for reasoning behind OMEGA slope choice]
Tuesday, May 02, 2017, 09:24
IGP1 = 2.34e-6 Torr
TBHT = 230A, 3.15V
TGHT = 298A, 3.96V
OMEGA = 1030C
Vacuum stable, increasing ramping rate up to 0.5A/min
Tuesday, May 02, 2017, 13:20
IGP1 = 1.3e-5 Torr
TGHT = 400A, 5.6V
OMEGA = 1175C
Increasing max setpoint to 500A
|
Wednesday, May 03, 2017, 13:33
TGHT had remained at 500A for 16hrs, vacuum had initially come down nicely.
Vacuum was starting to creep up when i came in this morning before 8am, IGP1 was at 1.2e-5 Torr
TGHT = 500A, 7.77V
OMEGA = 1440C
Around 8:30 vacuum started to spike, so the TGHT was tapped down rapidly to 450A
Tapping the TGHT down made no difference to the vacuum.
By the time 450A was hit, it was too late and the spike in vacuum caused the evaporator to trip off.
Turbo pump in epics showed on, turbo pump showed on according to TP direct controls.
Everything was shut off and the venting tapped, this made it obvious the turbo pump was already off as there was no ramping down noises from the turbo pump.
TP control box turned off then on again, at this point the controls showed a 'fail' message.
Turns out the turbo pump control box was fried and that's what had caused the turbo pump to fail with no notice in epics causing the vacuum to spontaneously spike.
Waiting on a new one from vacuum group...
See photos attached of striptool screenshots.
Wednesday, May 03, 2017, 15:03
New TP control boxed installed.
Turbo pump turned on, everything pumped down.
Vacuum good, IGP1 = 6.92e-7 Torr.
IGP2 still not working, won't turn on via epics.
Tried unplugging and plugging back in...still appears red with 'fail' message...
|
Wednesday, May 03, 2017, 16:07
Unplugging and plugging back in seemed to work now that evap2 under vacuum
IGP2 works again.
Will look into replacement ion gauge...
|
Wednesday, May 03, 2017, 16:09
HS water valves opened, no leaks detected.
Tapped up manually to 40A.
Vacuum stable.
IGP1 = 3.6e-7 Torr
Initiated auto-ramp at 1.0A/min and 0.5A/min to 300A and 230A for the TGHT and TBHT respectively.
Thursday, May 04, 2017, 08:41
Reached 300A, 230A 10hrs ago.
IGP1 = 1.5e-7 Torr
OMEGA = 1070C
Increasing max setpoint to 500A at a rate of 0.5A/min for TGHT
Thursday, May 04, 2017, 14:58
Back up to max setpoint that was reached before evap2 tripped off.
TGHT = 500A, 7.65V
IGP1 = 9.3e-7 Torr
OMEGA = 1450C
Increasing max setpoint to 550A, ramping up at a lower rate of 0.2A/min since this will be done overnight.
Friday, May 05, 2017, 08:53
TGHT = 550A, 8.64V
IGP1 = 2.8e-7 Torr
OMEGA = 1560C
Increasing max setpoint to 600A at a ramping rate of 0.5A/min
Friday, May 05, 2017, 11:09
TGHT = 600A, 9.58V
IGP1 = 7.3e-7 Torr
OMEGA = 1670C
Increasing max setpoint to 625A at a ramping rate of 0.5A/min
Friday, May 05, 2017, 12:05
TGHT = 625A, 10.05V
IGP1 = 9.9e-7 Torr
OMEGA = 1710C
Increasing max setpoint to 650A at a ramping rate of 0.5A/min
Friday, May 05, 2017, 13:13
TGHT = 650A, 10.57V
IGP1 = 1.1e-6 Torr
OMEGA = 1740C
Mikron through left side windown on outside bottom left edge on container = 1750C
Tapping up manually to 1800C
Friday, May 05, 2017, 13:42
Adjusted slope to 1.09 so same spot on leg using MIKRON = OMEGA
TGHT = 680A, 11.08V
IGP1 = 1.6e-6 Torr
OMEGA = 1795C
MIKRON = 1795C
Plotting a temperature curve, the predicted required current to reach 1800C was 670A using a slope of 1.08
Currently sitting 10A above predicted required current.
After several minutes, temperature dropped a few degrees to 1790C
Window remains clear and uncoated.
Tapped up to TGHT = 685A, 11.2V
OMEGA = 1795C
Will remain at this setpoint over the weekend.
Monday, May 08, 2017, 08:59
TGHT = 685A, 11.08V
TBHT = 230A, 3.24V
IGP1 = 1.98e-7 Torr
OMEGA has lowered to 1342C
Evap2 sat at max setpoints over the wknd.
Will check window port before cooling...
*UPDATE ON TRIP-OFF*
A closer look into the details using archives [see photos attached]:
TP tripped off TBHT and TGHT at ~8e-5Torr
Anything in the evaporator requires ~1hr to cool before turning things off.
In this scenario, the target was @ ~1440C. so ~30min post TP trip, the target may still be at ~1000C.
Anything above 0.02Torr could be close enough to atmopheric pressure that this would be cooling too fast and could lead to breaking the target/ cracking the Ta metal.
As one can see in the screenshots attached, the vacuum lingered around 0.005Torr for ~2hrs before anything was done.
This provided enough time for the target to cool before it was introduced to atmospheric pressure when the BV was closed when trying to figure out the problem.
In summary, the target 'should' be OK...will inspect target further when removed from the evaporator.
Tuesday, May 09, 2017, 09:16
TGHT = 685A, 11.04V
TGHT power supply = 686A, 11.31V
TBHT = 230A, 3.24V
TBHT power supply = 236A, 3.32V
IGP1 = 1.6e-7 Torr
IGP1 direct readout = 2.3e-7 mbar
IGP2 = 6.8e-8 Torr
IGP2 direct readout = 8.46e-8 Torr
Evap2 reached max setpoint friday afternoon.
Window clearly coated - see attached photo.
Initiating auto cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Wednesday, May 10, 2017, 09:18
Vented in air and opened up this morning.
Inspected container carefully for any cracks/ marks due to TP tripping off at 1450C
Target looks good!
One sample disc removed for SEM.
When removing disc for sample, the SiC came off the graphite backing and just SiC flake came out - see photo
Photos attached showing inside container with no Si crystal formation/ good clear path all the way through target and sample removed for tests
|
|
Thursday, May 11, 2017, 11:30, Laura Lambert, , , , Maintenance, New Ion Gauge for IGP2
|
Thursday, May 11, 2017, 11:25
IGP2 has been having problems where sometimes it turns off and requires simply unplugging and plugging back in.
Ion gauge has been replaced.
At first the vacuum box appeared red on epics and when attempting to reset everything nothing would work and the backing pump would try and turn on then timeout.
Apparently this new ion gauge draws slightly more than the old one and this blew a fuse in the PLC.
Old fuse was 2A, so a new 3A fuse has been replaced - seems to be working fine now.
|
Thursday, May 11, 2017, 11:25, Laura Lambert, Empty, 41369-10, HP-FEBIAD-CTL, Done, RUSH! Sintering TaC coated container for SiC#36
|
Thursday, May 11, 2017, 11:21
Turns out SiC HP-FEBIAD that has finished conditioning is loaded in the wrong container and it should be a SiC HP-FEBIAD cold transfer line...so rush on new target.
Container coated with TaC using new method: Ends taped off, with liquid poured in and swirled around entire container, then poured back out - 'flushing technique'
Container is wrapped with 1x heatshield around each side of cooling fins, not incl center block.
Loaded into EVAP2 and currently pumping down.
Thursday, May 11, 2017, 13:40
IGP1 = 1.85e-6 Torr.
HS water valves opened.
No leaks detected.
Tapped up manually to 35A.
Vacuum stable.
IGP1 = 3.2e-6 Torr
IGP2 = 4.2e-6 Torr
Initiated auto ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
Final setpoints for TGHT = 450A and TBHT = 230A, with final desired temp of 1900C
OMEGA slope = 0.98
Friday, May 12, 2017, 07:57
IGP1 = 4.3e-7 Torr.
IGP2 = 4.4e-7 Torr
TGHT = 233A, 2.8V
TBHT = 130A, 1.6V
Increasing ramping rate to 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Friday, May 12, 2017, 08:54
Comparing direct readouts with epics:
IGP1: direct = 1.9e-6 Torr; epics = 1.3e-6 Torr
IGP2: direct = 1.55e-6 Torr; epics = 1.4e-6 Torr
TGHT: direct = 320A, 4.38V; epics = 321A, 4.19V
TBHT: direct = 181A, 2.40V; epics = 178A, 2.34V
Friday, May 12, 2017, 10:28
IGP1 = 1.07e-6 Torr
IGP2 = 1.15e-6 Torr
TGHT = 450A, 6.37V
TBHT = 230A, 3.21V
OMEGA = 1197C
Increasing max setpoint of TGHT = 700A
Friday, May 12, 2017, 13:06
IGP1 = 2.4e-6 Torr
IGP2 = 2.5e-6 Torr
TGHT = 696A, 11.21V
TBHT = 233A, 3.26V
OMEGA = 1758C
Increasing max setpoint of TGHT = 800A
Friday, May 12, 2017, 13:32
TGHT maxed out at 715A but continued ramping.
This was noticed when current set of TGHT = 750A but readout = 715A
This is due to max voltage limit = 12.0V and readout =11.58V
Increasing TGHT max setpoint to 14.0V and restarting auto ramp from 714A
Friday, May 12, 2017, 14:45
Container has reached max setpoint of ~1900C
TGHT setpoint = 775A
TGHT = 769A, 12.54V
TBHT = 233A, 3.28V
IGP1 = 2.94e-6 Torr
IGP2 = 2.99e-6 Torr
OMEGA = 1912C
Will remain at max setpoint over weekend.
See attached photos of temperature measurements using MIKRON while TGHT current set point = 770A.
Photos are not super accurate but good as a rough idea.
Ex. for left side the point in the camera is actually pointed slightly closer to the end of the container but in the photo it looks more centered.
Saturday, May 13, 2017, 10:52 by Anders
Ramping down heaters. Temp 1912 C. Vacuum IGP1 = 5.4e-7 Torr
Monday, May 15, 2017, 13:10
Vented in air and taken out this a.m.
Target container looks good.
Fully sintered coating.
|
Wednesday, May 10, 2017, 16:07, Laura Lambert, Empty, , TARGET BOAT, In progress, Conditioning Heat Shield for IGLIS UCx#20 - test stand is down
|
Wednesday, May 10, 2017, 16:05
Loaded.
HS water valves opened, no leaks detected.
Started auto-ramp at a rate of 1A/30sec to a final setpoint of 580A
|
Wednesday, May 10, 2017, 21:33, Anders Mjos, Empty, , TARGET BOAT, In progress, Conditioning Heat Shield for IGLIS UCx#20 - test stand is down
|
Laura Lambert wrote: |
Wednesday, May 10, 2017, 16:05
Loaded.
HS water valves opened, no leaks detected.
Started auto-ramp at a rate of 1A/30sec to a final setpoint of 580A
|
Wednesday, May 10, 2017, 21:31: TGHT at 580 A for 1 h. Vacuum came down to 1.4E-6 Torr. TGHT voltage stable. Ramping down. |
Thursday, May 11, 2017, 10:51, Laura Lambert, Empty, , TARGET BOAT, Done, Conditioning Heat Shield for IGLIS UCx#20 - test stand is down
|
Anders Mjos wrote: |
Laura Lambert wrote: |
Wednesday, May 10, 2017, 16:05
Loaded.
HS water valves opened, no leaks detected.
Started auto-ramp at a rate of 1A/30sec to a final setpoint of 580A
|
Wednesday, May 10, 2017, 21:31: TGHT at 580 A for 1 h. Vacuum came down to 1.4E-6 Torr. TGHT voltage stable. Ramping down.
|
Thursday, May 11, 2017, 10:51
vented in air and opened it up this morning.
Heat shield looks good!
|
Monday, May 08, 2017, 10:05, Laura Lambert, , , , Maintenance, Turbo pump control box replaced
|
Monday, May 08, 2017, 10:05
Turbo pump control box died last week.
Replaced with a new one.
|
Thursday, April 20, 2017, 12:45, John Wong, np-SiC, , TARGET BOAT, In progress, Higher Temp Treament: B3-92Mpa pellets
|
Thursday, April 20, 2017, 12:38
3 samples are loaded into the Ta boat and wrapped with heat shield (1 long piece, 3 rounds): 2x of B3-92Mpa pellets and 10% pure PAN pellet as control. See lab book page 32 for more details.
The B3-92Mpa pellets were previously heated to 1550C (TGHT 400A/6.94V), see elog#351
Attempting to heat samples up to 1800C to determine the weight loss and shrinkage.
Est. TGHT 480A.
OK to auto ramp to 400A at 1A/min. Check for coating on the window.
Chamber is currently being pumped down.
Thursday, April 20, 2017, 14:28
Pressure 3.14e-6 Torr. Auto ramp TGHT at 1A/min to reach 400A.
Friday, April 21, 2017, 10:56
TGHT at 400A/6.75V, temp at 1475C (75C/0.19V lower).
Tapping up TGHT
Friday, April 21, 2017, 12:32
TGHT ramped up to 530A/9.85V, temp at 1800C.
Friday, April 21, 2017, 15:38
TGHT dropped slightly, no coating on windows.
Checked with Mikron, agreed with the dropped temp.
Tapped up TGHt to 545A/10.1V to reach 1800C. Will keep at that temp for several days.
Wednesday, April 26, 2017, 17:06
Samples have been heated at 1800C (-25C) for 7 days now (see attachment for archiver).
Cooling down TGHT at 1A/min.
|
Thursday, April 13, 2017, 12:03, Laura Lambert, SiC, , TARGET BOAT, Done, Sintering SiC pellets
|
Thursday, April 13, 2017, 12:01
Pellets made this morning and weighed.
Placed in a graphite boat which is placed inside a previously TaC coated boat.
Boat is wrapped with 3x Ta heat shields.
Loaded into evap2.
Chamber currently pumping down.
Tuesday, April 18, 2017, 13:53
HS water valves were opened this morning, no leaks detected.
Tapped up manually to 100A, 1.28V
Vacuum stable.
IGP1 = 3.63e-6 Torr.
Initiating auto ramp at a rate of 1.0A/min to 150A
Final desired temperature of 1100C
Tuesday, April 18, 2017, 14:57
TGHT = 150A, 2.08V
Still no temperature reading on OMEGA.
Vacuum stable, IGP1 = 1.16e-6 Torr.
Initiating auto ramp at the same rate of 1.0A/min up to 200A.
Tuesday, April 18, 2017, 15:56
TGHT = 200A, 2.91V
OMEGA = 990C
IGP1 = 8.59e-7 Torr
Tapping up manually to 1100C...
Wednesday, April 19, 2017, 08:34
TGHT = 235A, 3.47V
OMEGA = 1090C
IGP1 = 1.6e-7 Torr.
Has remained at ~1100C since 16:30 yesterday.
Intitiating auto-cool at 2.0A/min
Thursday, April 20, 2017, 08:40
Vented in air and taken out yesterday.
Pellets look good.
No obvious colour change.
|
Wednesday, April 05, 2017, 15:42, Laura Lambert, Empty, , TARGET BOAT, In progress, Sintering TaC coating on evap1 target boat
|
Wednesday, April 05, 2017, 15:36
Coated container with TaC coating using spray technique this morning and let dry.
Wrapped with one long layer of Ta heat shield, wrapped around boat 3x
No ends to target boat
Installed in evap2 and pumping down now...
|
Thursday, April 06, 2017, 08:57, Laura Lambert, Empty, , TARGET BOAT, Problems, Sintering TaC coating on evap1 target boat
|
Laura Lambert wrote: |
Wednesday, April 05, 2017, 15:36
Coated container with TaC coating using spray technique this morning and let dry.
Wrapped with one long layer of Ta heat shield, wrapped around boat 3x
No ends to target boat
Installed in evap2 and pumping down now...
|
Thursday, April 06, 2017, 08:56
Problems with IGP2
Won't turn on, has low voltage output.
See screenshot attached.
|
Thursday, April 06, 2017, 11:15, Laura Lambert, Empty, , TARGET BOAT, Problems resolved, Sintering TaC coating on evap1 target boat
|
Laura Lambert wrote: |
Laura Lambert wrote: |
Wednesday, April 05, 2017, 15:36
Coated container with TaC coating using spray technique this morning and let dry.
Wrapped with one long layer of Ta heat shield, wrapped around boat 3x
No ends to target boat
Installed in evap2 and pumping down now...
|
Thursday, April 06, 2017, 08:56
Problems with IGP2
Won't turn on, has low voltage output.
See screenshot attached.
|
Thursday, April 06, 2017, 11:12
Turns out it was just a bad connection.
See attached photos.
|
Thursday, April 06, 2017, 13:16, Laura Lambert, Empty, 40282-2, TARGET BOAT, Done, Sintering TaC coating on evap1 target boat
|
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Wednesday, April 05, 2017, 15:36
Coated container with TaC coating using spray technique this morning and let dry.
Wrapped with one long layer of Ta heat shield, wrapped around boat 3x
No ends to target boat
Installed in evap2 and pumping down now...
|
Thursday, April 06, 2017, 08:56
Problems with IGP2
Won't turn on, has low voltage output.
See screenshot attached.
|
Thursday, April 06, 2017, 11:12
Turns out it was just a bad connection.
See attached photos.
|
Thursday, April 06, 2017, 13:16
HS water valves opened, no leaks detected.
Tapped up manually to 35A
Waited almost 2hrs
IGP1 = 9.9e-7 Torr
Initiating auto-ramp at 0.2A/min to 400A
Final desired temperature = 1900C
OMEGA slope = 0.98
Good vac at 3.0e-5, bad vac at 4.0e-5 Torr.
Monday, April 10, 2017, 09:26
IGP1 = 1.79e-7 Torr
TGHT = 400A, 6.47V
OMEGA = 1505C
Tapping up manually to 1900C...
Monday, April 10, 2017, 11:46
TGHT tripped off at 410A, ~1530C
Water is still on and good flow.
Vacuum was stable ~1.8e-7 Torr.
No power trips according to controls.
Not sure of reasoning behind trip.
Initially tried tapping back-up, no current was being applied.
Turned off and back on TGHT power supply - this restarted things and now works again.
Have tapped back up to 35A, vacuum still good.
Restarting auto-ramp to 400A at 1.0A/min
Monday, April 10, 2017, 13:13
Vacuum looks good.
IGP1 = 1.1e-7 Torr
TGHT = 127A, 1.30V
Increasing ramping rate to 2.0A/min
Monday, April 10, 2017, 16:08
IGP1 = 1.5e-7 Torr
TGHT = 400A, 6.24V
OMEGA = 1510V
Increasing auto ramp setpoint to 450A at a rate of 0.2A/min
Wednesday, April 12, 2017, 11:06
IGP1 = 2.96e-7 Torr
TGHT = 555A, 9.74V
OMEGA = 1935C
Has remained at max setpoints overnight.
Initiating auto-cool at 2.0A/min
Thursday, April 13, 2017, 11:59
vented in air and opened up this morning.
container looks good.
see photo attached.
|
Friday, March 31, 2017, 12:22, John Wong, np-SiC, , TARGET BOAT, In progress, Thermo test: B3 Pellets (13.3K-PSI)
|
Friday, March 31, 2017, 12:21
Two compressed pellets loaded into the target boat and wrapped with Ta foil. (see lab book p32 for details).
Chamber is pumping down.
Desired temp 1550C, TGHT expected to be around 400A.
Friday, March 31, 2017, 16:31
Auto-ramp at 0.5A/min to reach 350A.
Saturday, April 01, 2017, 12:30
TGHT reached to 350A/5.7V, temp around 1200C - notice voltage is much lower than previous process (ID 351), possible target/heat shield shorted therefore lower temp observed. (This should not cause any damage to the container.)
Continue to ramp up to 400A. Notice some evolution of gasses similar to the previous process (ID351) during ramping up of TGHT around 220A . (see attachment1)
Saturday, April 01, 2017, 13:52
TGHT reached to 400A/6.7V; temp stabilized at 1400C.
Tap up to 1550, TGHT 456A/8.08V (3.7KW, about 1KW higher than before).
Pressure coming down (see attachment 2)
Hold temp for several days.
Saturday, April 01, 2017, 17:22
Temp went up by 10C. Lowered TGHT to 450A.
|
Monday, March 13, 2017, 15:34, Anders Mjos, Ta, 41790-4, LP-SIS, Done, Conditioning Ta#51
|
Target container wrapped in 3x heat shield foils and installed by JW
Monday, March 13, 2017, 15:33: Opened water for HS. Vacuum stable at IG1 1E-6 T
Monday, March 13, 2017, 15:48: TGHT / TBHT to 30 / 15 A.
Monday, March 13, 2017, 15:54: Started auto-ramping to TGHT / TBHT 150 / 75 A at 1 / 0.5 A/min. Good/bad vacuum 3 / 4 E-5 Torr
Tuesday, March 14, 2017, 08:23: Continue auto-ramping to TGHT / TBHT 300 / 150 A. Vacuum stable at IG1 2.3E-7 T
Tuesday, March 14, 2017, 11:18: Continue auto-ramping to TGHT / TBHT 350 / 200 A. Vacuum stable at IG1 3.8E-7 T
Wednesday, March 15, 2017, 08:31: Continue auto-ramping to TGHT 375. Vacuum stable at IG1 2.5E-7 T. Omega at 1500 C
Wednesday, March 15, 2017, 16:34: Continue auto-ramping to TGHT 500. Vacuum increased to IG1 5.5E-7 T. Omega at 1887 C
Thursday, March 16, 2017, 08:34: Continue auto-ramping to TGHT 520. Vacuum increased to IG1 3.3E-7 T. Omega at 1888 C
Thursday, March 16, 2017, 08:48: TGHT at 521 A 8.99 V. Omega at 1899 C
Friday, March 17, 2017, 08:25: TGHT at 521 A 8.88 V. Omega at 1886 C. Vacuum IG1 2.5E-7 Torr
Ramping down
Wednesday, March 22, 2017, 08:42: Turbo pump stopped |
Saturday, March 11, 2017, 11:58, John Wong, np-SiC, , TARGET BOAT, Done, Thermo test B3 Pellets
|
Friday, March 10, 2017, 17:29
Three B3 pellets are loaded into the container for thermo test.
(see lab book1 Pg 26, 28-30 for more detail about the materials)
Desired temp ~1500C; one long-sheet of Ta foil is used, est 400A.
Auto ramping 0.5A/min to 300A first. Check later...
Saturday, March 11, 2017, 11:58
Increased TGHT from 300A to 350A last night at ramping rate of 0.5A/min.
Tapped up further from 350A to 400A, 6.92V (2.8kW), Temp measured at ~1550C.
Pressure peaked at 1.5e-6 Torr and coming down when ramping TGHT from 350A to 400A. (see attachment1)
Will remain at the current. Continue monitoring..
Monday, March 13, 2017, 01:14
Temp was held at 1550C for about 1.5days. Vac stabilized at 3.08e-7 torr. TGHT 400A/6.94V.
Initiated cooling at 1A/min.
Next, Materials inspection.
Monday, March 13, 2017, 11:24
Target has been at room temp for about 4 hours. Venting chamber.
|
Tuesday, February 21, 2017, 15:21, Laura Lambert, Empty, 42218-1, LP-IG-LIS, Done, sintering TaC coating on UCx#20 container
|
Tuesday, February 21, 2017, 15:19
Container coated with TaC using 'flushing technique' and let dry overnight.
Cleaned ionizer tube with acetone, no coating inside ionizer tube
Wrapped with 3 x Ta heat shields, incl center block
Currently pumping down in evap2
OMEGA slope = 0.98
Good vac at 3.0e-5, bad vac at 4.0e-5 Torr.
Wednesday, February 22, 2017, 09:41
HS water valves opened, no leaks detected.
Tapped up manually to 35A
Waited ~45min
Vacuum stable.
IGP1 = 1.2e-6 Torr
Initiating auto ramp for TGHT @ 0.2A/min to a max setpoint of 350A
Initiating auto ramp for TBHT @ 0.1A/min to a max setpoint of 230A
Once max setpoints achieved, will tap up manually to final desired temperature of 1900C
Friday, February 24, 2017 by Anders
Continue manually to 1900 C
Friday, February 24, 2017, 16:24: TGHT at 400 A 6.35V IG1 = 4.5e-7 Torr 1660 C
Friday, February 24, 2017, 16:57: TGHT at 410 A 6.6 V IG1 = 5.0e-7 Torr 1700 C
Sunday, February 26, 2017 by Anders
Sunday, February 26, 2017, 14:13: TGHT at 425 A 6.9 V IG1 = 2.5e-7 Torr
Lab closed for weekend. No access to temp reading.
Monday, February 27, 2017, 16:12
Tapped up manually to 1900C this morning.
TGHT = 490A, 8.14V
TBHT = 230A, 2.98V
MIKRON = 1911C
OMEGA = 1904C
evap2 has remained at max setpoints for ~6hrs
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Tuesday, February 28, 2017, 11:57
Container finished sintering.
Vented in air and opened up this morning.
Container looks good
|
Friday, February 03, 2017, 14:18, Laura Lambert, Endcaps, , TARGET BOAT, Problems, Sintering TaC coating on Ta endcaps and springs
|
Friday, February 03, 2017, 14:17
The endcaps are stacked together with a punched out disc of graphite foil placed in between each endcap for separation so endcaps won't fuse together.
The end caps are further wrapped in a larger piece of graphite foil to hold together as a tube [same method used in elogID # 158 and 235]
There are also 4 coated springs, 2 on each side of the endcaps tube, with the endcaps tube residing in the middle of the boat.
The boat is wrapped with 3-layers of Ta heatshields.
Chamber is currently being pumped down.
Good vac at 3.0e-5, bad vac at 4.0e-5 Torr.
OMEGA slope = 0.98
Monday, February 06, 2017, 09:29
Power outage this weekend and evap2 tripped off.
Re-pumping down now...
Tuesday, February 07, 2017, 08:54
HS water valves opened, no leaks detected.
IGP1 = 1.9e-7 Torr
Tapped up manually to 35A
Vacuum stable.
IGP1 = 2.0e-7 Torr
Initiating auto-ramp at 0.2A/min with a final setpoint of 450A.
Final desired temperature = 1800C
Wednesday, February 08, 2017, 09:52
IGP1 = 2.98e-7 Torr
TGHT = 325A, 3.5V
Vacuum stable.
Increasing ramping rate to 1.0A/min
Wednesday, February 08, 2017, 11:46
IGP1 = 6.3e-7 Torr
TGHT = 433A, 4.89V
Increasing max setpoint to TGHT = 500A
OMEGA has still yet to show a temperature...should be reading points at this high in current
Will go down to the lab and follow up on OMEGA settings to confirm everything is set up ok before proceeding to a higher current...
Wednesday, February 08, 2017, 16:03
IGP1 = 4e-7 Torr
TGHT = 500A, 5.75V
OMEGA still not reading
Initiating auto-cool at -2A/min
Will update elog with more details tomorrow
Thursday, February 09, 2017, 10:52
Evap2 was cooled down and opened up this morning.
Turns out both legs on the target boat were touching the new heatshield and therefore had been loosing power.
Normally a boat at 500A would read ~1800C, in this scenario at 500A the boat read ~1000C.
A lot of power was being lost into the heatshield.
See photos attached of target boat sitting at 500A.
The heatshield is currently being ground down in those two spots to accommodate the target boat.
|
Tuesday, February 14, 2017, 15:44, Laura Lambert, Endcaps, , TARGET BOAT, Problems resolved, Sintering TaC coating on Ta endcaps and springs
|
Laura Lambert wrote: |
Friday, February 03, 2017, 14:17
The endcaps are stacked together with a punched out disc of graphite foil placed in between each endcap for separation so endcaps won't fuse together.
The end caps are further wrapped in a larger piece of graphite foil to hold together as a tube [same method used in elogID # 158 and 235]
There are also 4 coated springs, 2 on each side of the endcaps tube, with the endcaps tube residing in the middle of the boat.
The boat is wrapped with 3-layers of Ta heatshields.
Chamber is currently being pumped down.
Good vac at 3.0e-5, bad vac at 4.0e-5 Torr.
OMEGA slope = 0.98
Monday, February 06, 2017, 09:29
Power outage this weekend and evap2 tripped off.
Re-pumping down now...
Tuesday, February 07, 2017, 08:54
HS water valves opened, no leaks detected.
IGP1 = 1.9e-7 Torr
Tapped up manually to 35A
Vacuum stable.
IGP1 = 2.0e-7 Torr
Initiating auto-ramp at 0.2A/min with a final setpoint of 450A.
Final desired temperature = 1800C
Wednesday, February 08, 2017, 09:52
IGP1 = 2.98e-7 Torr
TGHT = 325A, 3.5V
Vacuum stable.
Increasing ramping rate to 1.0A/min
Wednesday, February 08, 2017, 11:46
IGP1 = 6.3e-7 Torr
TGHT = 433A, 4.89V
Increasing max setpoint to TGHT = 500A
OMEGA has still yet to show a temperature...should be reading points at this high in current
Will go down to the lab and follow up on OMEGA settings to confirm everything is set up ok before proceeding to a higher current...
Wednesday, February 08, 2017, 16:03
IGP1 = 4e-7 Torr
TGHT = 500A, 5.75V
OMEGA still not reading
Initiating auto-cool at -2A/min
Will update elog with more details tomorrow
Thursday, February 09, 2017, 10:52
Evap2 was cooled down and opened up this morning.
Turns out both legs on the target boat were touching the new heatshield and therefore had been loosing power.
Normally a boat at 500A would read ~1800C, in this scenario at 500A the boat read ~1000C.
A lot of power was being lost into the heatshield.
See photos attached of target boat sitting at 500A.
The heatshield is currently being ground down in those two spots to accommodate the target boat.
|
Tuesday, February 14, 2017, 15:43
Heatshield was ground back and target boat now fits nicely into heatshield without contact.
|
Tuesday, February 14, 2017, 15:48, Laura Lambert, Endcaps, , TARGET BOAT, Done, Sintering TaC coating on Ta endcaps and springs
|
Laura Lambert wrote: |
Laura Lambert wrote: |
Friday, February 03, 2017, 14:17
The endcaps are stacked together with a punched out disc of graphite foil placed in between each endcap for separation so endcaps won't fuse together.
The end caps are further wrapped in a larger piece of graphite foil to hold together as a tube [same method used in elogID # 158 and 235]
There are also 4 coated springs, 2 on each side of the endcaps tube, with the endcaps tube residing in the middle of the boat.
The boat is wrapped with 3-layers of Ta heatshields.
Chamber is currently being pumped down.
Good vac at 3.0e-5, bad vac at 4.0e-5 Torr.
OMEGA slope = 0.98
Monday, February 06, 2017, 09:29
Power outage this weekend and evap2 tripped off.
Re-pumping down now...
Tuesday, February 07, 2017, 08:54
HS water valves opened, no leaks detected.
IGP1 = 1.9e-7 Torr
Tapped up manually to 35A
Vacuum stable.
IGP1 = 2.0e-7 Torr
Initiating auto-ramp at 0.2A/min with a final setpoint of 450A.
Final desired temperature = 1800C
Wednesday, February 08, 2017, 09:52
IGP1 = 2.98e-7 Torr
TGHT = 325A, 3.5V
Vacuum stable.
Increasing ramping rate to 1.0A/min
Wednesday, February 08, 2017, 11:46
IGP1 = 6.3e-7 Torr
TGHT = 433A, 4.89V
Increasing max setpoint to TGHT = 500A
OMEGA has still yet to show a temperature...should be reading points at this high in current
Will go down to the lab and follow up on OMEGA settings to confirm everything is set up ok before proceeding to a higher current...
Wednesday, February 08, 2017, 16:03
IGP1 = 4e-7 Torr
TGHT = 500A, 5.75V
OMEGA still not reading
Initiating auto-cool at -2A/min
Will update elog with more details tomorrow
Thursday, February 09, 2017, 10:52
Evap2 was cooled down and opened up this morning.
Turns out both legs on the target boat were touching the new heatshield and therefore had been loosing power.
Normally a boat at 500A would read ~1800C, in this scenario at 500A the boat read ~1000C.
A lot of power was being lost into the heatshield.
See photos attached of target boat sitting at 500A.
The heatshield is currently being ground down in those two spots to accommodate the target boat.
|
Tuesday, February 14, 2017, 15:43
Heatshield was ground back and target boat now fits nicely into heatshield without contact.
|
Tuesday, February 14, 2017, 15:44
Boat with endcaps and springs reloaded today and pumped back down this afternoon.
HS water valves opened, no leaks detected.
Tapped up manually to 35A
Vacuum stable.
IGP1 = 3.5e-6 Torr
Initiating auto-ramp at 0.2A/min with a final setpoint of 400A.
Final desired temperature = 1800C
Wednesday, February 15, 2017, 10:24
IGP1 = 7.2e-7 Torr
TGHT = 260A, 3.95V
OMEGA = 1158C
Vacuum stable.
Increasing ramping rate to 1.0A/min.
Wednesday, February 15, 2017, 13:02
IGP1 = 2.0e-6 Torr
TGHT = 400A, 6.67V
OMEGA = 1530C
Increasing final setpoint to 450A
Wednesday, February 15, 2017, 13:55
IGP1 = 2.5e-6 Torr
TGHT =450A, 7.7V
OMEGA = 1640C
Increasing final setpoint to 500A
Wednesday, February 15, 2017, 15:13
IGP1 = 1.8e-6 Torr
TGHT = 500A, 8.59V
OMEGA = 1770C
MIKRON = 1740C
Tapping up manually to ~1800C...
Thursday, February 16, 2017, 09:09
IGP1 = 5.28e-7 Torr
TGHT = 520A, 9.1V
OMEGA = 1821C
Target boat has remained at max setpoints for 17.5hrs.
Initiating auto-cool at 1A/min
Thursday, February 16, 2017, 13:49
Increasing auto-cool to 2.0A/min
Friday, February 17, 2017, 16:00
Vented in air and opened up today.
Endcaps looks good see photos attached
|
Thursday, February 09, 2017, 23:28, John Wong, np-SiC, , TARGET BOAT, Done, Thermotest: SiC-SiO2-Lys and SiC pellets
|
Thursday, February 09, 2017, 23:26
There are two types of samples being test for thermal stability:
1. SiC-SiO2-Lys nanofiber mats
2. SiC pellets
(see Lab Book for more info)
Desired temperature: ~1500C
One-Ta heat shield is used, est. TGHT 450A.
Thursday, February 09, 2017, 23:38
TGHT currently at 322A/5.28V, OMEGA 1204C.
Vac 2.9e-6 Torr.
Friday, February 10, 2017, 08:58
TGHT at 400A, temp at 1425C for 8 hours.
Decided to cool down for analysis. Check for carboreduction for SiO2 at 1400C. Then continue to ramp up to 1500C.
Ramping down at 2A/min
Friday, February 10, 2017, 10:47
Rapid out-gas (2.7e-6 to 3.8e-6 Torr) from TGHT 330A until current stopped at 400A (see attachment). Could be the evolution of O2 from SiO2...
|
Thursday, February 09, 2017, 11:49, Laura Lambert, , , , Maintenance, New heatshield with flexible water lines
|
Thursday, February 09, 2017, 11:47
A new heatshield with flexible water lines has been put into evap2 last Friday Feb3rd
|
Monday, February 06, 2017, 11:17, Anders Mjos, , , , Problems resolved, IOC restart after power outagae
|
Dave Morris did a remote restart of the IOC after the outage. Turbo pump started. |
Tuesday, January 31, 2017, 16:03, Laura Lambert, Empty, 39530-10, HP-FEBIAD, Done, Sintering TaC coated container for backup
|
Tuesday, January 31, 2017, 13:43
Container coated with TaC using new method: Ends taped off, with liquid poured in and swirled around entire container, then poured back out - 'flushing technique'
Container is wrapped with 3 x Ta heat shields, not incl center block.
Loaded into EVAP2 and currently pumping down.
Tuesday, January 31, 2017, 16:02
IGP1 = 3.9e-6 Torr.
HS water valves opened.
No leaks detected.
Tapped up manually to 35A.
Vacuum stable.
Initiated auto ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
Final setpoints for TGHT = 450A and TBHT = 230A, with final desired temp of 1900C
OMEGA slope = 0.98
Wednesday, February 01, 2017, 10:01
IGP1 = 5.7e-7 Torr.
TGHT = 254A, 3.0V
TBHT = 142A, 1.8V
Increasing ramping rate to 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Wednesday, February 01, 2017, 11:48
IGP1 = 1.7e-6 Torr.
TGHT = 450A, 6.27V
TBHT = 230A, 3.14V
OMEGA = 1176C
Increasing max setpoint of TGHT = 600A
Wednesday, February 01, 2017, 13:09
IGP1 = 3.7e-6 Torr.
TGHT = 600A, 9.0V
TBHT = 230A, 3.18V
OMEGA = 1480C
Increasing max setpoint of TGHT = 700A
Wednesday, February 01, 2017, 14:08
IGP1 = 3.8e-6 Torr.
TGHT = 700A, 10.96V
TBHT = 230A, 3.2V
OMEGA = 1705C
Increasing max setpoint of TGHT = 750A
Wednesday, February 01, 2017, 15:02
IGP1 = 5.1e-6 Torr.
TGHT = 750A, 11.87V
TBHT = 230A, 3.2V
OMEGA = 1808C
Increasing max setpoint of TGHT = 800A
Wednesday, February 01, 2017, 15:30
IGP1 = 6.6e-6 Torr.
TGHT = 800A, 12.86V
TBHT = 230A, 3.2V
OMEGA = 1903C
Will remain at max setpoints overnight.
Thursday, February 02, 2017, 09:16
Remained at max setpoints for ~18hrs.
IGP1 = 9.5e-7 Torr.
OMEGA =1914C
TGHT = 800A, 12.83V
TBHT = 230A, 3.22V
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Friday, February 03, 2017, 14:24
Vented in air and opened up this morning
Coating looks good.
See photos attached.
|
Tuesday, December 20, 2016, 15:04, Laura Lambert, , , , Maintenance, RETURN and SUPPLY valves CLOSED for xmas break
|
Tuesday, December 20, 2016, 15:05
confirmed ~full tank of Ar for glove box --> ~1600psi |
Friday, December 16, 2016, 14:14, Laura Lambert, Ta, 39530-3, LP-FEBIAD, Done, Conditioning Ta FEBIAD target for shutdown tests
|
Friday, December 16, 2016, 14:08
Target consists of 470 discs.
Total packed length 3.4cm [exactly 7.8cm space on both sides]
Total mass 45.9091g [Incl foils + Ta wire on 6 packs]
Target consists of 350 single discs and 6x20 packs of Ta discs
Discs in target are arranged as follows: 1pack / 75singles / 1pack / 100singles / 2packs / 100singles / 1pack / 75singles / 1pack
3x Ta Heat shields.
LP-FEBIAD container with large center block.
No endcaps inserted, no Rh foil inserted.
Chamber currently pumping down.
TBHT will be ramped up to 230A at 1.0A/min.
TGHT will be ramped up to 350A at 2.0A/min.
Final desired temperature = 1900C
Friday, December 16, 2016, 14:32
HS water valves opened, no leaks detected
Tapped up manually to 35A
Vacuum stable, IGP1 = 2.1e-6 Torr
Initiating auto-ramp.
OMEGA slope = 0.98
Monday, December 19, 2016, 11:52
Tapped up manually to ~1900C [see attached excel for details on data collected - interesting temperature fluctuations]
Will remain at max setpoints for min 4hrs then auto-cool
Monday, December 19, 2016, 15:20
Target has remained at max setpoints for just over 4hrs
TGHT = 520A, 8.67V
OMEGA = 1820C
IGP1 = 5.2e-7 Torr
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Tuesday, December 20, 2016, 11:52
Vented in air and opened up this morning.
Looks like the windows was coated in evap2, unsure if this was missed and coated before conditioning target or if this is from materials coming out during conditioning process...
Target looks good.
Endcaps inserted but not expanded.
|
Thursday, December 01, 2016, 16:08, Laura Lambert, Empty, 42218-12, LP-SIS, Done, sintering TaC coating on UCx#19 container
|
Thursday, December 01, 2016, 16:06
Container coated with TaC using 'flushing technique' and let dry overnight.
Cleaned ionizer tube with acetone, no coating inside ionizer tube
Wrapped with 3 x Ta heat shields, incl center block
Currently pumping down in evap2
OMEGA slope = 0.98
Friday, December 02, 2016, 11:24
Opened up HS water valves, no leaks detected.
Tapped up manually to 35A.
Waited ~25min, vacuum stable.
IGP1 = 1.65e-6 Torr
Initiating auto-ramp at 0.2A/min for the TGHT and 0.1A/min for the TBHT.
Max setpoints set for 350A and 230A for the TGHT and TBHT respectively.
Once max setpoints achieved, will tap up manually to final desired temperature of 1900C
Monday, December 05, 2016, 09:38
TGHT = 350A, 5.38V
TBHT = 230A, 4.03V
OMEGA = 1550C
IGP1 = 3.2e-7 Torr
Tapping up to 1900C...
Monday, December 05, 2016, 14:11
OMEGA = 1905C
TGHT = 475A, 7.63V
TBHT = 230A, 4.07V
IGP1 = 8.5e-7 Torr
Tuesday, December 06, 2016, 08:41
TGHT = 475A, 7.76V
TBHT = 230A, 4.07V
IGP1 = 3.9e-7 Torr
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Wednesday, December 07, 2016, 08:46
Evap2 was vented in air and opened up yesterday afternoon.
Container looks good, coating fully sintered.
|
Tuesday, November 22, 2016, 15:58, Laura Lambert, Nb, 40282-3, TARGET BOAT, Done, Conditioning Nb samples for Doug
|
Tuesday, November 22, 2016, 15:53
Target boat has a layer of niobium foil on the bottom of the boat.
A niobium foil has been made with slots to hold samples [similar to when sintering endcaps] *See attached photos
Niobium samples are placed in slots, holding in place, to avoid warping.
Smaller samples closest to MIKRON IR reading [left side]
Boat is wrapped with 1 large layer of Ta foil, wrapped around the boat 3x, careful to avoid touching samples.
Loaded into evap2 today.
Pumping down now...
Wednesday, November 23, 2016, 11:45
HS water valves opened, no leaks detected.
Tapped up manually to 35A.
IGP1 = 6.4e-7 Torr
Setting auto-ramp rate at 0.2A/min to max setpoint of 250A.
Will tap up manually to final desired temperature of 1400C.
Wednesday, November 23, 2016, 13:17
IGP1 = 5.9e-7
TGHT = 66A, 0.51V
Vacuum stable.
Increasing ramping rate to 1.0A/min
Thursday, November 24, 2016, 08:46
IGP1 = 3.9e-7 Torr
TGHT = 250A, 3.41V *NOTE: the current set reads 243.8A but the readout is 250A
OMEGA = 1013C
MIKRON has no reading yet
Tapping up manually to 1400C
Thursday, November 24, 2016, 15:42
Samples have remained at ~1400C for 5hrs.
IGP1 = 5.8e-7 Torr
TGHT = 420A, 6.5V
OMEGA = 1410C
MIKRON = 1420C
Initiating auto-cool at 2.0A/min
Friday, November 25, 2016, 11:39
Vented in air and opened up this morning.
Samples look good!
|
Tuesday, November 15, 2016, 16:51, John Wong, np-SiC, , TARGET BOAT, In progress, Heat-treatment: Beta-SiC (1um) fiber mats - SAMPLE ID: A1
|
Tuesday, November 15, 2016, 16:48
Three samples were prepared (see my logbook#1 page 3, preparing for carbonization).
One layer of Ta foil was used to wrap around the target boat.
Chamber is currently being pumped down
Wednesday, November 16, 2016, 11:04
Ramping up TGHT at 2A/min, set at 350A.
Desired temperature, ~1530C (similar heating condition as raw npSiC heat treatment, elog ID335)
Thursday, November 17, 2016, 10:09
TGHT reached to 350A/5.80V, stayed for over 20 hours. Temp measured at 1276 C (Mikon) and 1270 (Omega), vac at 6.07e-7 Torr.
Stepping up TGHT to reach the desired temp.
|
Thursday, November 17, 2016, 11:15, Laura Lambert, np-SiC, , TARGET BOAT, In progress, Heat-treatment: Beta-SiC (1um) fiber mats - SAMPLE ID: A1
|
John Wong wrote: |
Tuesday, November 15, 2016, 16:48
Three samples were prepared (see my logbook#1 page 3, preparing for carbonization).
One layer of Ta foil was used to wrap around the target boat.
Chamber is currently being pumped down
Wednesday, November 16, 2016, 11:04
Ramping up TGHT at 2A/min, set at 350A.
Desired temperature, ~1530C (similar heating condition as raw npSiC heat treatment, elog ID335)
Thursday, November 17, 2016, 10:09
TGHT reached to 350A/5.80V, stayed for over 20 hours. Temp measured at 1276 C (Mikon) and 1270 (Omega), vac at 6.07e-7 Torr.
Stepping up TGHT to reach the desired temp.
|
Thursday, November 17, 2016, 11:13
TGHT = 400A, 6.73V
IGP1 = 8.2e-7 Torr
OMEGA = 1385C
MIKRON = 1389C
Tapping up manually to 1500C or a max setpoint of 450A
Thursday, November 17, 2016, 11:56
TGHT = 450A, 7.85V
IGP1 = 1.7e-6 Torr
OMEGA = 1502C
MIKRON = 1510C
Friday, November 18, 2016, 10:08
IGP1 = 5.3e-7 Torr
TGHT = 450A, 7.9V
OMEGA = 1510C
MIKRON = 1515C
Evap2 has remained at max setpoints for 23hrs.
Initiating auto-cool at 2.0A/min
|
Friday, November 18, 2016, 17:28, John Wong, np-SiC, , TARGET BOAT, Done, Heat-treatment: Beta-SiC (1um) fiber mats - SAMPLE ID: A1
|
Laura Lambert wrote: |
John Wong wrote: |
Tuesday, November 15, 2016, 16:48
Three samples were prepared (see my logbook#1 page 3, preparing for carbonization).
One layer of Ta foil was used to wrap around the target boat.
Chamber is currently being pumped down
Wednesday, November 16, 2016, 11:04
Ramping up TGHT at 2A/min, set at 350A.
Desired temperature, ~1530C (similar heating condition as raw npSiC heat treatment, elog ID335)
Thursday, November 17, 2016, 10:09
TGHT reached to 350A/5.80V, stayed for over 20 hours. Temp measured at 1276 C (Mikon) and 1270 (Omega), vac at 6.07e-7 Torr.
Stepping up TGHT to reach the desired temp.
|
Thursday, November 17, 2016, 11:13
TGHT = 400A, 6.73V
IGP1 = 8.2e-7 Torr
OMEGA = 1385C
MIKRON = 1389C
Tapping up manually to 1500C or a max setpoint of 450A
Thursday, November 17, 2016, 11:56
TGHT = 450A, 7.85V
IGP1 = 1.7e-6 Torr
OMEGA = 1502C
MIKRON = 1510C
Friday, November 18, 2016, 10:08
IGP1 = 5.3e-7 Torr
TGHT = 450A, 7.9V
OMEGA = 1510C
MIKRON = 1515C
Evap2 has remained at max setpoints for 23hrs.
Initiating auto-cool at 2.0A/min
|
Friday, November 18, 2016, 17:27
The heat treatment of the fiber mats is done.
Analyzing steps...
|
Monday, October 24, 2016, 17:52, John Wong, np-SiC, , TARGET BOAT, Done, Thermo test of np-SiC raw powder
|
Monday, October 24, 2016, 17:43
Two samples were prepared and loaded into the target boat with 1 layer of heat-shied as shown in the attachment#1.
Ingredients used: np-SiC and very small about of 5% PVA to hold the powder together.
Samples were dried in the oven at 110C before loaded in Evap#2.
After dried:
Sample #1 (larger graphite boat, mass =0.3779) = 0.4259g (PVA mass unknown due to solution leaking out from the boat)
Sample #2 = 0.2306g (with 5% PVA of 0.4111g)
Test temperature at 1600C, expect TGHT to be around 400A.
Monday, October 24, 2016, 17:50
Ramping up TGHT to 300A at 0.5A/min. Vac at 2.3e-6 Torr.
Tuesday, October 25, 2016, 12:59
TGHT reached to 300A and stabilized for 10 hours. OMEGA temp reader at 1150C
Continue to ramp up TGHT
Wednesday, October 26, 2016, 15:49
TGHT was ramped up to 450A/7.91V; the temp readers on MIKON and OMEGA were 1489 and 1535, respectively (see attachment).
The temperature was much lower than the previous two tests (see elog #296 and #335). Not sure why...
Will do composition analysis on the sample...
Cooling down at 2A/min.
|
Thursday, October 13, 2016, 18:05, Laura Lambert, Ta, 41790-5, LP-SIS, In progress, Temperature measurements for Ta#50
|
Thursday, October 13, 2016, 18:04
Target loaded into evap2
No heat shields.
Both endcaps inserted and expanded.
Rh foil inserted [when inserting, the Ta rod used to expand the Rh foil inside the ionizer tube snapped off inside the container - this piece was able to be shaken out and is no longer inside]
Chamber pumped down.
HS water valves opened, no leaks detected
Tapped up manually to 35A
Vacuum stable, IGP1 = 5e-7 Torr
Initiating auto-ramp.
OMEGA slope = 0.98
TBHT will be ramped up to 230A at 1.0A/min.
TGHT will be ramped up to 300A at 2.0A/min.
Final desired temperature = 1900C
Friday, October 14, 2016, 13:28
TGHT and TBHT had reached 300A/ 230A respectively.
Power bump ~10min ago caused evap2 to trip off.
Tapped back up manually to 35A.
Re-initiating auto ramp now.
|
Saturday, October 15, 2016, 12:42, Aurelia Laxdal, Ta, 41790-5, LP-SIS, In progress, Temperature measurements for Ta#50
|
Laura Lambert wrote: |
Thursday, October 13, 2016, 18:04
Target loaded into evap2
No heat shields.
Both endcaps inserted and expanded.
Rh foil inserted [when inserting, the Ta rod used to expand the Rh foil inside the ionizer tube snapped off inside the container - this piece was able to be shaken out and is no longer inside]
Chamber pumped down.
HS water valves opened, no leaks detected
Tapped up manually to 35A
Vacuum stable, IGP1 = 5e-7 Torr
Initiating auto-ramp.
OMEGA slope = 0.98
TBHT will be ramped up to 230A at 1.0A/min.
TGHT will be ramped up to 300A at 2.0A/min.
Final desired temperature = 1900C
Friday, October 14, 2016, 13:28
TGHT and TBHT had reached 300A/ 230A respectively.
Power bump ~10min ago caused evap2 to trip off.
Tapped back up manually to 35A.
Re-initiating auto ramp now.
|
Friday October 14: the target was ramp up to 300A/230A after Laura started it. Then, I cooled down at 6pm before leaving TRIUMF. <br>
Saturday October 15: restated the auto-ramp for Ta#50 in EVAP2. It's currently set to go to 300A/230A. |
Sunday, October 16, 2016, 17:55, Aurelia Laxdal, Ta, 41790-5, LP-SIS, In progress, Temperature measurements for Ta#50
|
Aurelia Laxdal wrote: |
Laura Lambert wrote: |
Thursday, October 13, 2016, 18:04
Target loaded into evap2
No heat shields.
Both endcaps inserted and expanded.
Rh foil inserted [when inserting, the Ta rod used to expand the Rh foil inside the ionizer tube snapped off inside the container - this piece was able to be shaken out and is no longer inside]
Chamber pumped down.
HS water valves opened, no leaks detected
Tapped up manually to 35A
Vacuum stable, IGP1 = 5e-7 Torr
Initiating auto-ramp.
OMEGA slope = 0.98
TBHT will be ramped up to 230A at 1.0A/min.
TGHT will be ramped up to 300A at 2.0A/min.
Final desired temperature = 1900C
Friday, October 14, 2016, 13:28
TGHT and TBHT had reached 300A/ 230A respectively.
Power bump ~10min ago caused evap2 to trip off.
Tapped back up manually to 35A.
Re-initiating auto ramp now.
|
Friday October 14: the target was ramp up to 300A/230A after Laura started it. Then, I cooled down at 6pm before leaving TRIUMF. <br>
Saturday October 15: restated the auto-ramp for Ta#50 in EVAP2. It's currently set to go to 300A/230A.
|
Sunday October 16: the target temperature measurements up to 620A/230A were performed today not on October 15 (yesterday, it was cooled down before reaching 300A/230A). Currently the target is cooling down, to be ready tomorrow morning for the Test Stand. |
Tuesday, October 18, 2016, 09:23, Laura Lambert, Ta, 41790-5, LP-SIS, Done, Temperature measurements for Ta#50
|
Aurelia Laxdal wrote: |
Aurelia Laxdal wrote: |
Laura Lambert wrote: |
Thursday, October 13, 2016, 18:04
Target loaded into evap2
No heat shields.
Both endcaps inserted and expanded.
Rh foil inserted [when inserting, the Ta rod used to expand the Rh foil inside the ionizer tube snapped off inside the container - this piece was able to be shaken out and is no longer inside]
Chamber pumped down.
HS water valves opened, no leaks detected
Tapped up manually to 35A
Vacuum stable, IGP1 = 5e-7 Torr
Initiating auto-ramp.
OMEGA slope = 0.98
TBHT will be ramped up to 230A at 1.0A/min.
TGHT will be ramped up to 300A at 2.0A/min.
Final desired temperature = 1900C
Friday, October 14, 2016, 13:28
TGHT and TBHT had reached 300A/ 230A respectively.
Power bump ~10min ago caused evap2 to trip off.
Tapped back up manually to 35A.
Re-initiating auto ramp now.
|
Friday October 14: the target was ramp up to 300A/230A after Laura started it. Then, I cooled down at 6pm before leaving TRIUMF. <br>
Saturday October 15: restated the auto-ramp for Ta#50 in EVAP2. It's currently set to go to 300A/230A.
|
Sunday October 16: the target temperature measurements up to 620A/230A were performed today not on October 15 (yesterday, it was cooled down before reaching 300A/230A). Currently the target is cooling down, to be ready tomorrow morning for the Test Stand.
|
Monday, October 17, 2016, 09:21
Vented in air and taken out this morning.
Target looks good!
|
Friday, October 07, 2016, 16:42, Laura Lambert, Ta, 41790-5, LP-SIS, In progress, Conditioning Ta#50
|
Friday, October 07, 2016, 16:40
Target consists of 470 discs.
Total packed length 3.4cm [exactly 7.8cm space on both sides]
Total mass 47.6889g [Incl foils + Ta wire on 6 packs]
Note: Target consists of 350 single discs and 6x20 packs of Ta discs
3x Ta Heat shields.
No endcaps inserted, no Rh foil inserted.
Chamber currently pumping down.
TBHT will be ramped up to 230A at 1.0A/min.
TGHT will be ramped up to 300A at 2.0A/min.
Final desired temperature = 1900C
Tuesday, October 11, 2016, 10:02
HS water valves opened, no leaks detected
Tapped up manually to 35A
Vacuum stable, IGP1 = 2e-7 Torr
Initiating auto-ramp.
OMEGA slope = 0.98
Wednesday, October 12, 2016, 16:15
Tapped up to 1900C? [see attached link for data concerning temperature readings]
TGHT = 450A, 7.16V
TBHT = 230A, 4.1V
OMEGA = 1748C
IGP1 = 6.1e-7 Torr
|
Wednesday, October 12, 2016, 21:18, John Wong, Ta, 41790-5, LP-SIS, In progress, Conditioning Ta#50
|
Laura Lambert wrote: |
Friday, October 07, 2016, 16:40
Target consists of 470 discs.
Total packed length 3.4cm [exactly 7.8cm space on both sides]
Total mass g [Incl foils + Ta wire on 6 packs]
Note: Target consists of 350 single discs and 6x20 packs of Ta discs
3x Ta Heat shields.
No endcaps inserted, no Rh foil inserted.
Chamber currently pumping down.
TBHT will be ramped up to 230A at 1.0A/min.
TGHT will be ramped up to 300A at 2.0A/min.
Final desired temperature = 1900C
Tuesday, October 11, 2016, 10:02
HS water valves opened, no leaks detected
Tapped up manually to 35A
Vacuum stable, IGP1 = 2e-7 Torr
Initiating auto-ramp.
OMEGA slope = 0.98
Wednesday, October 12, 2016, 16:15
Tapped up to 1900C? [see attached link for data concerning temperature readings]
TGHT = 450A, 7.16V
TBHT = 230A, 4.1V
OMEGA = 1748C
IGP1 = 6.1e-7 Torr
|
Wednesday, October 12, 2016, 21:14
Current status before cooling down:
TGHT at 450A/7.32V; TBHT at 230A/4.10V; OMEGA at 1747C
Vacuum at 4.05 e-7 Torr.
Initiate auto-rampping at 2A/min for TGHT and 1A/min for TBHT
|
Thursday, October 13, 2016, 17:32, Laura Lambert, Ta, 41790-5, LP-SIS, Done, Conditioning Ta#50
|
John Wong wrote: |
Laura Lambert wrote: |
Friday, October 07, 2016, 16:40
Target consists of 470 discs.
Total packed length 3.4cm [exactly 7.8cm space on both sides]
Total mass g [Incl foils + Ta wire on 6 packs]
Note: Target consists of 350 single discs and 6x20 packs of Ta discs
3x Ta Heat shields.
No endcaps inserted, no Rh foil inserted.
Chamber currently pumping down.
TBHT will be ramped up to 230A at 1.0A/min.
TGHT will be ramped up to 300A at 2.0A/min.
Final desired temperature = 1900C
Tuesday, October 11, 2016, 10:02
HS water valves opened, no leaks detected
Tapped up manually to 35A
Vacuum stable, IGP1 = 2e-7 Torr
Initiating auto-ramp.
OMEGA slope = 0.98
Wednesday, October 12, 2016, 16:15
Tapped up to 1900C? [see attached link for data concerning temperature readings]
TGHT = 450A, 7.16V
TBHT = 230A, 4.1V
OMEGA = 1748C
IGP1 = 6.1e-7 Torr
|
Wednesday, October 12, 2016, 21:14
Current status before cooling down:
TGHT at 450A/7.32V; TBHT at 230A/4.10V; OMEGA at 1747C
Vacuum at 4.05 e-7 Torr.
Initiate auto-rampping at 2A/min for TGHT and 1A/min for TBHT
|
Thursday, October 13, 2016, 17:32
vented in air and opened up this morning.
target looks good. |
Wednesday, September 28, 2016, 17:09, Laura Lambert, Empty, 41790-6, LP-SIS, Done, sintering TaC coating on UCx container
|
Wednesday, September 28, 2016, 17:08
Container coated with TaC using 'flushing technique' today, cleaned ionizer tube with acetone, no coating inside ionizer tube
Dried by blowing air into tube
Wrapped with 3 x Ta heat shields, incl center block - new method of each layer being one long single Ta foil covering entire container incl center block
Currently pumping down in evap2
Thursday, September 29, 2016, 11:11
HS water valves opened
Tapped up to 35A
Waited ~45min, vacuum stable
IGP1 = 1.4e-6 Torr
Initiating auto ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
Max setpoints for TGHT = 350A and TBHT = 230A
Once max setpoints achieved, will tap up manually to final desired temperature of 1900C
Friday, September 30, 2016, 10:51
IGP1 = 7.8e-7 Torr
TGHT = 315A, 4.57V
TBHT = 174A, 2.8V
Increasing ramping rate to 1.0A/min and 0.5A/min for the TGHT and TBHT respectively.
Friday, September 30, 2016, 11:44
Changed OMEGA slope to 0.98
IGP1 = 1e-6 Torr
TGHT = 350A, 5.2V
TBHT = 201A, 3.4V
Increasing ramping rate of TBHT to 1.0A/min
OMEGA = 1625C / MIKRON = 1625C
Friday, September 30, 2016, 15:45
IGP1 = 1.1e-6 Torr
TGHT = 430A, 6.79V
TBHT = 230A, 4.07V
OMEGA = 1903C
Will remain at max setpoints over weekend.
See attached link for raw data of manual tap up.
Also see attached photos of screenshots showing oval - not circular - tube of target container at two different temperatures...
Monday, October 03, 2016, 13:28
IGP1 = 1.79e-7 Torr
TGHT = 430A, 6.87V
TBHT = 230A, 4.06V
OMEGA = 1892C
MIKRON = 1847C
Attached is a picture taken through the MIKRON, the slight oval shape appears to be a minor bend in the target container:
With the ionizer tube facing into the page, the bend appears to be in the center with both ends of the container bent slightly towards the page
This possible bend in the container gives the appearance of the oval shape through the camera while it is being heated, due to the angle of the camera
Remained at max setpoints over weekend.
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Tuesday, October 04, 2016, 13:40
Vented in air and opened up this morning.
Container done, TaC coating looks good.
Waiting further inspection...
Tuesday, October 04, 2016, 14:48
Container placed on jig and inspected.
Approved to go ahead for use online by Anders and Friedhelm.
|
Thursday, September 15, 2016, 16:37, Laura Lambert, SiC, 39530-9, HP-FEBIAD, In progress, Sintering SiC#35
|
Thursday, September 15, 2016, 16:23
Target container contains 487 discs of SiC
Target packed length = 16cm.
Mass of SiC(green) = 58.8795g
Container is wrapped with 1x heatshield around each side of cooling fins; no end caps are inserted yet - coated spring inserted both sides to hold discs in place.
Sintering temp = 1800C
Chamber is currently being pumped down.
Friday, September 16, 2016, 10:50
Tapped up manually to 50A
Waited ~1hr , vacuum stable.
IGP1 = 1.24e-5 Torr
Initiating auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
TGHT max = 500A. TBHT max at 230A.
Slope on OMEGA = 1.15
Monday, September 19, 2016, 10:53
OMEGA = 1230C
TGHT = 360A, 4.75V
TBHT = 204A, 2.68V
IGP1 = 5.3e-6 Torr
Increasing ramping rate to 1.0A/min and 0.5A/min for the TGHT and TBHT respectively.
Monday, September 19, 2016, 11:57
OMEGA = ~1300C
TBHT = 230A, 3.16V
TGHT = 409A, 5.55V
Lowering ramping rate to 0.2A/min while vaccum high
IGP1 = 3.05e-5 Torr
Monday, September 19, 2016, 13:22
OMEGA = 1350C
TGHT = 425A, 5.82V
IGP1 = 1.97e-5 Torr
Stepping ramping rate back up to 1.0A/min
|
Monday, September 19, 2016, 18:48, John Wong, SiC, 39530-9, HP-FEBIAD, In progress, Sintering SiC#35 - Change OMEGA/MiKRON slopes
|
Laura Lambert wrote: |
Thursday, September 15, 2016, 16:23
Target container contains 487 discs of SiC
Target packed length = 16cm.
Mass of SiC(green) = 58.8795g
Container is wrapped with 1x heatshield around each side of cooling fins; no end caps are inserted yet - coated spring inserted both sides to hold discs in place.
Sintering temp = 1800C
Chamber is currently being pumped down.
Friday, September 16, 2016, 10:50
Tapped up manually to 50A
Waited ~1hr , vacuum stable.
IGP1 = 1.24e-5 Torr
Initiating auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
TGHT max = 500A. TBHT max at 230A.
Slope on OMEGA = 1.15
Monday, September 19, 2016, 10:53
OMEGA = 1230C
TGHT = 360A, 4.75V
TBHT = 204A, 2.68V
IGP1 = 5.3e-6 Torr
Increasing ramping rate to 1.0A/min and 0.5A/min for the TGHT and TBHT respectively.
Monday, September 19, 2016, 11:57
OMEGA = ~1300C
TBHT = 230A, 3.16V
TGHT = 409A, 5.55V
Lowering ramping rate to 0.2A/min while vaccum high
IGP1 = 3.05e-5 Torr
Monday, September 19, 2016, 13:22
OMEGA = 1350C
TGHT = 425A, 5.82V
IGP1 = 1.97e-5 Torr
Stepping ramping rate back up to 1.0A/min
|
Monday, September 19, 2016, 18:24
Measuring the temperature on the SiC is difficult due to the changing in emissivity as the temperature goes up. So, I will use the MIKRON to measure the temperature on the Ta surface near the end of the tube and OMEGA for measuring the inside.
Using the analogue pyrometer, the temperature on the Ta surface at the end of the tube was measured at around ~1450C; this temperature match the temperature on the Mikron at slope 0.98 (as usual). To match it with OMEGA, I changed the slope to 1.04 since this measurement is taking readings on the inside of the tube and on the SiC material.
Note: The measurements are NOT the absolute temperature. These are relative temperature measurements which give some guideline where the target current should be at for the sintering process. Please plot the temp vs current as the TGHT is being ramped up. At some point, the windows will get coated and the measurement is no longer reliable. The plot will be used to give an estimation of the current for 1800C.
|
Tuesday, September 20, 2016, 15:40, Laura Lambert, SiC, 39530-9, HP-FEBIAD, In progress, Sintering SiC#35
|
John Wong wrote: |
Laura Lambert wrote: |
Thursday, September 15, 2016, 16:23
Target container contains 487 discs of SiC
Target packed length = 16cm.
Mass of SiC(green) = 58.8795g
Container is wrapped with 1x heatshield around each side of cooling fins; no end caps are inserted yet - coated spring inserted both sides to hold discs in place.
Sintering temp = 1800C
Chamber is currently being pumped down.
Friday, September 16, 2016, 10:50
Tapped up manually to 50A
Waited ~1hr , vacuum stable.
IGP1 = 1.24e-5 Torr
Initiating auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
TGHT max = 500A. TBHT max at 230A.
Slope on OMEGA = 1.15
Monday, September 19, 2016, 10:53
OMEGA = 1230C
TGHT = 360A, 4.75V
TBHT = 204A, 2.68V
IGP1 = 5.3e-6 Torr
Increasing ramping rate to 1.0A/min and 0.5A/min for the TGHT and TBHT respectively.
Monday, September 19, 2016, 11:57
OMEGA = ~1300C
TBHT = 230A, 3.16V
TGHT = 409A, 5.55V
Lowering ramping rate to 0.2A/min while vaccum high
IGP1 = 3.05e-5 Torr
Monday, September 19, 2016, 13:22
OMEGA = 1350C
TGHT = 425A, 5.82V
IGP1 = 1.97e-5 Torr
Stepping ramping rate back up to 1.0A/min
|
Monday, September 19, 2016, 18:24
Measuring the temperature on the SiC is difficult due to the changing in emissivity as the temperature goes up. So, I will use the MIKRON to measure the temperature on the Ta surface near the end of the tube and OMEGA for measuring the inside.
Using the analogue pyrometer, the temperature on the Ta surface at the end of the tube was measured at around ~1450C; this temperature match the temperature on the Mikron at slope 0.98 (as usual). To match it with OMEGA, I changed the slope to 1.04 since this measurement is taking readings on the inside of the tube and on the SiC material.
Note: The measurements are NOT the absolute temperature. These are relative temperature measurements which give some guideline where the target current should be at for the sintering process. Please plot the temp vs current as the TGHT is being ramped up. At some point, the windows will get coated and the measurement is no longer reliable. The plot will be used to give an estimation of the current for 1800C.
|
Tuesday, September 20, 2016, 15:18
there was a temperature fluctuation resulting in the MIKRON no longer matching the readout on the OMEGA
this prompted another change in the slope on the OMEGA to 1.08
TGHT was then tapped up manually to 600A/ 1800C
will remain at this max setpoint for a few days before ramping down
see attachment for raw data
Wednesday, September 21, 2016, 11:34
temperatures dropped a small amount overnight.
tapped up manually to 625A/ 1810C
still no coating on window.
see attachment for updated raw data
|
Thursday, September 22, 2016, 12:14, John Wong, SiC, 39530-9, HP-FEBIAD, In progress, Sintering SiC#35
|
Laura Lambert wrote: |
John Wong wrote: |
Laura Lambert wrote: |
Thursday, September 15, 2016, 16:23
Target container contains 487 discs of SiC
Target packed length = 16cm.
Mass of SiC(green) = 58.8795g
Container is wrapped with 1x heatshield around each side of cooling fins; no end caps are inserted yet - coated spring inserted both sides to hold discs in place.
Sintering temp = 1800C
Chamber is currently being pumped down.
Friday, September 16, 2016, 10:50
Tapped up manually to 50A
Waited ~1hr , vacuum stable.
IGP1 = 1.24e-5 Torr
Initiating auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
TGHT max = 500A. TBHT max at 230A.
Slope on OMEGA = 1.15
Monday, September 19, 2016, 10:53
OMEGA = 1230C
TGHT = 360A, 4.75V
TBHT = 204A, 2.68V
IGP1 = 5.3e-6 Torr
Increasing ramping rate to 1.0A/min and 0.5A/min for the TGHT and TBHT respectively.
Monday, September 19, 2016, 11:57
OMEGA = ~1300C
TBHT = 230A, 3.16V
TGHT = 409A, 5.55V
Lowering ramping rate to 0.2A/min while vaccum high
IGP1 = 3.05e-5 Torr
Monday, September 19, 2016, 13:22
OMEGA = 1350C
TGHT = 425A, 5.82V
IGP1 = 1.97e-5 Torr
Stepping ramping rate back up to 1.0A/min
|
Monday, September 19, 2016, 18:24
Measuring the temperature on the SiC is difficult due to the changing in emissivity as the temperature goes up. So, I will use the MIKRON to measure the temperature on the Ta surface near the end of the tube and OMEGA for measuring the inside.
Using the analogue pyrometer, the temperature on the Ta surface at the end of the tube was measured at around ~1450C; this temperature match the temperature on the Mikron at slope 0.98 (as usual). To match it with OMEGA, I changed the slope to 1.04 since this measurement is taking readings on the inside of the tube and on the SiC material.
Note: The measurements are NOT the absolute temperature. These are relative temperature measurements which give some guideline where the target current should be at for the sintering process. Please plot the temp vs current as the TGHT is being ramped up. At some point, the windows will get coated and the measurement is no longer reliable. The plot will be used to give an estimation of the current for 1800C.
|
Tuesday, September 20, 2016, 15:18
there was a temperature fluctuation resulting in the MIKRON no longer matching the readout on the OMEGA
this prompted another change in the slope on the OMEGA to 1.08
TGHT was then tapped up manually to 600A/ 1800C
will remain at this max setpoint for a few days before ramping down
see attachment for raw data
Wednesday, September 21, 2016, 11:34
temperatures dropped a small amount overnight.
tapped up manually to 625A/ 1810C
still no coating on window.
see attachment for updated raw data
|
Thursday, September 22, 2016, 12:07
Temperature reader on OMEGA dropped slightly to 1785C overnight. The temperature on the leg remained at 1800C (MIKRON). No coating on windows.
Increased TGHT to 635A/10.12V (local 10.40V). OMEGA reads 1800C, MIKRON ~1817C.
Continue to monitor… (see dropbox for captured photos)
|
Monday, September 26, 2016, 13:49, Laura Lambert, SiC, 39530-9, HP-FEBIAD, Done, Sintering SiC#35
|
John Wong wrote: |
Laura Lambert wrote: |
John Wong wrote: |
Laura Lambert wrote: |
Thursday, September 15, 2016, 16:23
Target container contains 487 discs of SiC
Target packed length = 16cm.
Mass of SiC(green) = 58.8795g
Container is wrapped with 1x heatshield around each side of cooling fins; no end caps are inserted yet - coated spring inserted both sides to hold discs in place.
Sintering temp = 1800C
Chamber is currently being pumped down.
Friday, September 16, 2016, 10:50
Tapped up manually to 50A
Waited ~1hr , vacuum stable.
IGP1 = 1.24e-5 Torr
Initiating auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
TGHT max = 500A. TBHT max at 230A.
Slope on OMEGA = 1.15
Monday, September 19, 2016, 10:53
OMEGA = 1230C
TGHT = 360A, 4.75V
TBHT = 204A, 2.68V
IGP1 = 5.3e-6 Torr
Increasing ramping rate to 1.0A/min and 0.5A/min for the TGHT and TBHT respectively.
Monday, September 19, 2016, 11:57
OMEGA = ~1300C
TBHT = 230A, 3.16V
TGHT = 409A, 5.55V
Lowering ramping rate to 0.2A/min while vaccum high
IGP1 = 3.05e-5 Torr
Monday, September 19, 2016, 13:22
OMEGA = 1350C
TGHT = 425A, 5.82V
IGP1 = 1.97e-5 Torr
Stepping ramping rate back up to 1.0A/min
|
Monday, September 19, 2016, 18:24
Measuring the temperature on the SiC is difficult due to the changing in emissivity as the temperature goes up. So, I will use the MIKRON to measure the temperature on the Ta surface near the end of the tube and OMEGA for measuring the inside.
Using the analogue pyrometer, the temperature on the Ta surface at the end of the tube was measured at around ~1450C; this temperature match the temperature on the Mikron at slope 0.98 (as usual). To match it with OMEGA, I changed the slope to 1.04 since this measurement is taking readings on the inside of the tube and on the SiC material.
Note: The measurements are NOT the absolute temperature. These are relative temperature measurements which give some guideline where the target current should be at for the sintering process. Please plot the temp vs current as the TGHT is being ramped up. At some point, the windows will get coated and the measurement is no longer reliable. The plot will be used to give an estimation of the current for 1800C.
|
Tuesday, September 20, 2016, 15:18
there was a temperature fluctuation resulting in the MIKRON no longer matching the readout on the OMEGA
this prompted another change in the slope on the OMEGA to 1.08
TGHT was then tapped up manually to 600A/ 1800C
will remain at this max setpoint for a few days before ramping down
see attachment for raw data
Wednesday, September 21, 2016, 11:34
temperatures dropped a small amount overnight.
tapped up manually to 625A/ 1810C
still no coating on window.
see attachment for updated raw data
|
Thursday, September 22, 2016, 12:07
Temperature reader on OMEGA dropped slightly to 1785C overnight. The temperature on the leg remained at 1800C (MIKRON). No coating on windows.
Increased TGHT to 635A/10.12V (local 10.40V). OMEGA reads 1800C, MIKRON ~1817C.
Continue to monitor… (see dropbox for captured photos)
|
Monday, September 26, 2016, 13:24
Temperature decreased over weekend.
MIKRON dropped from ~1800C to ~1670C, OMEGA on right side remained ~1800C
Comparing screen shots of temperature readings and camera looking at target from left side, changes can be seen:
-darker area on top edge of target tube, above inside tube, grows larger when temperature drops - indicating 'cooler area' has grown
-initially darker area covers top above target materials on tube, when drops to ~1670C darker area extends down sides of target tube and reaches past target material area
See attached picture showing these details
Target has remained at this max setpoint for ~4-5 days
Windows remain un-coated.
Current and voltage readings remain un-changed.
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Wednesday, September 28, 2016, 17:05
Vented in air, target taken out today.
Target looks good!
A small amount of material was removed from the windows in evap2, very thin layer of coating.
Will update tomorrow with photos
Endcaps inserted.
|
Wednesday, September 07, 2016, 15:02, John Wong, Empty, 39530-9, HP-SIS, In progress, Sintering TaC coating container for SiC Target
|
Wednesday, September 07, 2016, 14:45
Container was previously coated with TaC solution and wrapped with 1-full length layer of Ta- heat shield around the fins.
Chamber is being pumped down. Vac at 5.6e-7 Torr before HS water valves were open; no leaks were detected.
Sintering Temperature 1900C (Omega slope @ 0.98); expected TGHT ~765A/11.90V, TGHT max at 230A.
Thursday, September 08, 2016, 18:14
At about 1600C, it was observed that the coating inside the tube seems to chip off (see attachment 1).
TGHT was ramped up to 745A/11.85V and TBHT to 230A/3.25V. Temperature measured on OMEGA/Mikron = 1914C/1881C; both instruments slopes set at 0.98.
Will remain at this TGHT current over night
Vac at 3.0e-6 Torr and coming down.
Friday, September 09, 2016, 11:01
Target has been heated at the stable temperature at 1914C (for OMEGA) and 1881C (for Mikron) with current at 745A/11.94V (see attachment 2) for almost 19 hours.
No fluctuation in p/s current or temperature was observed. The ramping up process is captured and can be view from the link below:
https://www.dropbox.com/sh/9lgtin54o17ds6j/AABn1-XjvK44mm74TjqTAmvta?dl=0
Pressure at 1.07e-6 Torr.
Cooling down TGHT at 2A/min and TBHT at 1A/min.
Continue to capture the cooling down process.
Friday, September 09, 2016, 15:17
While the target container was cooling down, the chip-like particle began obvious (see attachment 3).
Will inspect the container.. TGHT currently at 260A.
|
Monday, September 12, 2016, 17:22, John Wong, Empty, 39530-9, HP-SIS, Failed, TaC coating chipped off
|
John Wong wrote: |
Wednesday, September 07, 2016, 14:45
Container was previously coated with TaC solution and wrapped with 1-full length layer of Ta- heat shield around the fins.
Chamber is being pumped down. Vac at 5.6e-7 Torr before HS water valves were open; no leaks were detected.
Sintering Temperature 1900C (Omega slope @ 0.98); expected TGHT ~765A/11.90V, TGHT max at 230A.
Thursday, September 08, 2016, 18:14
At about 1600C, it was observed that the coating inside the tube seems to chip off (see attachment 1).
TGHT was ramped up to 745A/11.85V and TBHT to 230A/3.25V. Temperature measured on OMEGA/Mikron = 1914C/1881C; both instruments slopes set at 0.98.
Will remain at this TGHT current over night
Vac at 3.0e-6 Torr and coming down.
Friday, September 09, 2016, 11:01
Target has been heated at the stable temperature at 1914C (for OMEGA) and 1881C (for Mikron) with current at 745A/11.94V (see attachment 2) for almost 19 hours.
No fluctuation in p/s current or temperature was observed. The ramping up process is captured and can be view from the link below:
https://www.dropbox.com/sh/9lgtin54o17ds6j/AABn1-XjvK44mm74TjqTAmvta?dl=0
Pressure at 1.07e-6 Torr.
Cooling down TGHT at 2A/min and TBHT at 1A/min.
Continue to capture the cooling down process.
Friday, September 09, 2016, 15:17
While the target container was cooling down, the chip-like particle began obvious (see attachment 3).
Will inspect the container.. TGHT currently at 260A.
|
Monday, September 12, 2016, 16:54
The TaC coating chipped off from the surface and didn't get sintered with the container. (See attachment1).
There are a few possible reasons why this happened:
1. The coating was too think. This may cause the TaC layer to curl up while the heater was ramped up.
2. The coated material got brittle. The container was flushed with TaC (probably a few weeks ago?) before it went through the sintering process. Prolong exposure to air/light usually degrade the polymers viscoelasticity.
3. TaC solution has got bad. The particles can agglomerate over time and this can cause uneven surface.
4. Combination of all... ???
Anyway, the chipped off TaC layer was gently scraped off with a stainless steel rod. Then using kimwipes, i was able to remove most of the chipped off coating; it was not easy - especially trying to remove it from the inner tube.
Instead of "flushing" the tube with TaC, I decided to spray it with thin layer. And using the air supply, I could quickly dry the coating and installed it back to the evaporator for 2nd Round sintering as we are approaching the deadline!
. |
Monday, September 12, 2016, 17:27, John Wong, Empty, 39530-9, HP-SIS, Done, RUSH. Round 2: Sinering TaC coating
|
John Wong wrote: |
John Wong wrote: |
Wednesday, September 07, 2016, 14:45
Container was previously coated with TaC solution and wrapped with 1-full length layer of Ta- heat shield around the fins.
Chamber is being pumped down. Vac at 5.6e-7 Torr before HS water valves were open; no leaks were detected.
Sintering Temperature 1900C (Omega slope @ 0.98); expected TGHT ~765A/11.90V, TGHT max at 230A.
Thursday, September 08, 2016, 18:14
At about 1600C, it was observed that the coating inside the tube seems to chip off (see attachment 1).
TGHT was ramped up to 745A/11.85V and TBHT to 230A/3.25V. Temperature measured on OMEGA/Mikron = 1914C/1881C; both instruments slopes set at 0.98.
Will remain at this TGHT current over night
Vac at 3.0e-6 Torr and coming down.
Friday, September 09, 2016, 11:01
Target has been heated at the stable temperature at 1914C (for OMEGA) and 1881C (for Mikron) with current at 745A/11.94V (see attachment 2) for almost 19 hours.
No fluctuation in p/s current or temperature was observed. The ramping up process is captured and can be view from the link below:
https://www.dropbox.com/sh/9lgtin54o17ds6j/AABn1-XjvK44mm74TjqTAmvta?dl=0
Pressure at 1.07e-6 Torr.
Cooling down TGHT at 2A/min and TBHT at 1A/min.
Continue to capture the cooling down process.
Friday, September 09, 2016, 15:17
While the target container was cooling down, the chip-like particle began obvious (see attachment 3).
Will inspect the container.. TGHT currently at 260A.
|
Monday, September 12, 2016, 16:54
The TaC coating chipped off from the surface and didn't get sintered with the container. (See attachment1).
There are a few possible reasons why this happened:
1. The coating was too think. This may cause the TaC layer to curl up while the heater was ramped up.
2. The coated material got brittle. The container was flushed with TaC (probably a few weeks ago?) before it went through the sintering process. Prolong exposure to air/light usually degrade the polymers viscoelasticity.
3. TaC solution has got bad. The particles can agglomerate over time and this can cause uneven surface.
4. Combination of all... ???
Anyway, the chipped off TaC layer was gently scraped off with a stainless steel rod. Then using kimwipes, i was able to remove most of the chipped off coating; it was not easy - especially trying to remove it from the inner tube.
Instead of "flushing" the tube with TaC, I decided to spray it with thin layer. And using the air supply, I could quickly dry the coating and installed it back to the evaporator for 2nd Round sintering as we are approaching the deadline!
.
|
Monday, September 12, 2016, 17:24
Chamber was pumped down to low 10e-6 Torr before HS water valves were open - no leaks detected.
TGHT/TBHT auto ramped at 2A/min to 600A/230A.
Will continue to monitor..
Wednesday, September 14, 2016, 17:04
TGHT was stepped up to 700A and temp 1851C (OMEGA), 1930C(Mikron). (see attachment 1). The container was heated over night before it was cool down at 2A/min.
Target container seems to properly sintered with TaC (see attachment 2); it will be used for SiC#35.
|
Monday, August 08, 2016, 15:22, Laura Lambert, SiC, 40860-3, LP-IG-LIS, Problems, Conditioning SiC#34
|
Monday, August 08, 2016, 15:19
Previously sintered over weekend [see elog i.d 311]
Target container contains 471 discs of SiC [6 x 5 packs + 441 single discs]
Target packed length = 16cm.
Mass of 533 discs SiC(green) = 52.7172g
Container is wrapped with 3 heatshields; no end caps are inserted yet - coated spring inserted both sides to hold discs in place.
Conditioning temp = 1800C.
TGHT max = 450A. TBHT max = 230A.
Chamber is currently being pumped down.
Monday, August 08, 2016, 16:38
Target was not removed from evap2 after sintering, vented and cleaned windows only.
IGP1 = 5.5e-6 Torr
Stepped up manually to 80A, vacuum stable.
IGP1 = 3.2e-6 Torr
Initiating auto-ramp at 0.2A/min for the TGHT and 0.1A/min for the TBHT.
Thursday, August 11, 2016, 14:14
Tues the TGHT reached ~280A via auto-ramp
Evap2 was then tapped up manually to 480A/ ~1800C
Temperature readings on OMEGA have fluctuated up and down during conditioning process which was also observed for SiC#33
Also consistent with SiC#33, a lower current was required to reach 1800C during the conditioning process compared to the sintering process.
See attached link for data.
Tuesday, August 16, 2016, 16:25
TGHT remained at 480A, 9.2V for ~7 days.
IGP1 = 6.5e-6 Torr
OMEGA = 1470C [with window coating, so temperature reading compromised]
Initiating auto cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Wednesday, August 17, 2016, 13:40
Vented in air and opened this morning.
Target broke
Target clearly heated to high.
See attached snapshot of striptool from conditioning process.
Will update later with photos of broken container
|
Tuesday, August 30, 2016, 15:25, John Wong, SiC, 40860-3, LP-IG-LIS, Problems, Conditioning SiC#34. Note about the p/s voltage
|
Laura Lambert wrote: |
Monday, August 08, 2016, 15:19
Previously sintered over weekend [see elog i.d 311]
Target container contains 471 discs of SiC [6 x 5 packs + 441 single discs]
Target packed length = 16cm.
Mass of 533 discs SiC(green) = 52.7172g
Container is wrapped with 3 heatshields; no end caps are inserted yet - coated spring inserted both sides to hold discs in place.
Conditioning temp = 1800C.
TGHT max = 450A. TBHT max = 230A.
Chamber is currently being pumped down.
Monday, August 08, 2016, 16:38
Target was not removed from evap2 after sintering, vented and cleaned windows only.
IGP1 = 5.5e-6 Torr
Stepped up manually to 80A, vacuum stable.
IGP1 = 3.2e-6 Torr
Initiating auto-ramp at 0.2A/min for the TGHT and 0.1A/min for the TBHT.
Thursday, August 11, 2016, 14:14
Tues the TGHT reached ~280A via auto-ramp
Evap2 was then tapped up manually to 480A/ ~1800C
Temperature readings on OMEGA have fluctuated up and down during conditioning process which was also observed for SiC#33
Also consistent with SiC#33, a lower current was required to reach 1800C during the conditioning process compared to the sintering process.
See attached link for data.
Tuesday, August 16, 2016, 16:25
TGHT remained at 480A, 9.2V for ~7 days.
IGP1 = 6.5e-6 Torr
OMEGA = 1470C [with window coating, so temperature reading compromised]
Initiating auto cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Wednesday, August 17, 2016, 13:40
Vented in air and opened this morning.
Target broke
Target clearly heated to high.
See attached snapshot of striptool from conditioning process.
Will update later with photos of broken container
|
Tuesday, August 30, 2016, 15:17
A better look at the p/s voltage over the course of the constant heating at 480A. (see attachment).
The striptool shows the voltage was not giving a stable output. There were multiple occasions that the voltage dropped and then recovered; the obvious was on Aug 16. This indicates that the target was breaking up.
Finally on Aug 17, the voltage dropped and never recovered again - that indicates the target was broken. |
Wednesday, August 24, 2016, 17:07, John Wong, SiC, 39814-V2-1, LP-IG-LIS, Done, Sintering process for SiC#34 (2nd round) 10x
|
Wednesday, August 24, 2016, 17:05
Target container was previously coated with TaC and sintered up to 1900C at 420A/7.01V
Container is loaded with beta-SiC 432 discs at 16cm in length.
Container is wrapped with Ta-heat shield; no end-caps are used at this time.
Chamber is being pumped down.
Thursday, August 25, 2016, 12:04
Chamber has been pumped down overnight. Pressure at 5.9e-7 Torr.
HS water valve opened; no leaks were detected.
Sintering temperature 1800C. TGHT will be set accordingly to get the desired temperature. TBHT max at 230A.
Thursday, August 25, 2016, 12:12
Tapped up TGHT/TBHT to 40A. Vac at 7e-6 and slowly going up but still below limit.
Monday, August 29, 2016, 11:04
TGHT and TBHT reached to 250A (3.65V)//230A(3.02V), respectively, and kept stable over the weekend.
Temp measured at 1372C with slope set at 1.04 (1230C at slope 0.98).
No visible coating on windows.
Setting up TGHT to reach 1800C; monitoring locally
Monday, August 29, 2016, 14:35
Stepped up TGHT to 390A/6.54V; light coating was observed on the windows. The temperature should be around 1800C which should be in line with the power (current) deposited in the container during the TaC coat sintering process (1900A at 420A); however, with the light coating the reading may be off.
Mikron was used to measured inside of the tube (away from the discs); temperature was measured at ~1800C, (see attachment) [adjusted slope at 1.00 to compensate the SiC disc and Ta]
Omega was used to measured the temperature of the discs. It is difficult to know what's the temperature inside the tube, so this measurement is only taken as a guideline. Slope changed from 1.04 to 1.15 to match Mikron's reading.
After heated at 390A for 30 mins, the windows are now coated. Temp reading is no longer reliable. The temperature could be above 1800C. Keeping a close monitor!!!
No blockage inside the tube was observed.
Will remain heating at 390A/6.44V for overnight before proceeding with the re-conditioning.
Tuesday, August 30, 2016, 10:41
Target was heated at 390A for over 10 hours and then cool down at 1A/min (see attachment#2). Windows were fully coated and Omega couldn't register any reading.
Chamber will be vented and target will be inspected before proceeding with the re-conditioning step.
Tuesday, August 30, 2016, 12:13
Target was inspected; no visible damage was observed (see attachment)
Material coated on the windows and the cu heat shields; all parts were wiped off with acetone.
No visible material build up inside the container.
Chamber is now being pumped down for re-conditiing.
Tuesday, August 30, 2016, 13:05
HS water valves open; no leaks detected.
Vac at 3.6 e-6 Torr.
Ready to set up TGHT/TBHT
Tuesday, August 30, 2016, 16:41
TGHT/TBHT stepped up to 340A (5.40V) /230A (3.1V), respectively.
Temperature was measured at 1835C at TGHT of 340A. Omega, Mikron and analogue pyrometer were all reading ~1800C inside the tube (not on the SiC surface). For that reason, I decided to stop the current at 340A, instead of 390A.
TGHT voltage is running stable.
No visible coating or blockage inside the tube was observed.
Wednesday, August 31, 2016, 11:53
A thin layer of coating is observed on both the side windows (see attachment 5). The temp reading is no longer reliable.
TGHT remains at 340A/5.45V. P/S voltage is performing steadily.
No clogging inside the tube is observed.
Setting up another Omega reader to measure temperature from the front window since this window is clear and won't get coated (see attachment #6).
Temperature measurement from the front window is ~1140C; this corresponds to the measurement from the analogue pyrometer with the correction of e=~0.2 for tantalum at 1100C.
Note: The temperature measurements should be taken as relative. Since the reading from the side windows isn't reliable any longer, the centre window will give some information how stable the temperature is holding during the reconditioning process. Continue to monitor.
Wednesday, August 31, 2016, 16:24
About two hours ago, I increased TGHT to 350A and stayed there for a few mins (see attachment 7). No change in temp was observed - that's mainly due to the coating on the windows. As for the temp measurement from the center window, a more power current input would require to see the change as heat is slowly propagating through the layers of Ta heatshields.
Local inspection on the target: no clogging inside the tube. Voltage/Current is stable at 340A/5.45V. Vac at 1.43e-7 Torr.
Wednesday, August 31, 2016, 23:00
Strange observation: Temperature readers on both omega have gone up. (see attachment 8).
I'm not sure if the temperature is reiiable. I actually saw the increase in temperature ~1850C last night around the same time; no change in TGHT current/voltage. By the next morning, it went back down to 1400C with significant coating on the windows.
Wednesday, August 31, 2016, 23:28
I had ISAC Op (Justin) to help me go into the Hotlab and take a look at the reading on Mikron. Indeed, it is reading about 2000C which is close to the Omega reading. He also looked into the tube through Mikron scope and found no clogging inside the tube.
To be safe, I am going to lower the TGHT heater down to reach ~1800C.
Wednesday, August 31, 2016, 23:41
Lower TGHT to 305A/4.81V; OMEGA reading at 1830C. Vac at 1.27e-7 Torr. Will remain at this current over night.
Thursday, September 01, 2016, 12:16
Checked on the target.
Temperature readings, right windows (omega)= 1726C, centre = 1100C (omega), left (Mikron) = 1720C.
No blockage inside the tube.
TGHT stabilizes at 305A/4.79V. Vac at 1.09e-7 Torr.
Thursday, September 01, 2016, 16:32
About an hour ago, the temp dropped to 1660C with no change in TGHT current/voltage (see attachment 9).
Vac is a 1.06e-7 Torr.
After consulting with Friedhelm, we decided to cool the target down and inspect it tomorrow.
Ramping TGHT/TBHT at 2A/min.
Wednesday, September 07, 2016, 15:13
The target was removed from the Evap and inspected.
Some spots on both ends and ionizer tube were crystalized. (see attachment 10).
No blockage inside the tube was observed.
End caps were inserted.
The target was assembled and tested - All seems fine.
|
Wednesday, August 17, 2016, 17:31, Laura Lambert, Empty, 39814-V2-1, LP-IG-LIS, In progress, sintering TaC coating on SiC#34 container...round2
|
Wednesday, August 17, 2016, 17:30
Container coated with TaC using 'flushing technique', cleaned ionizer tube with acetone, so no coating inside ionizer tube
Wrapped with 3 x Ta heat shields, incl center block
Currently pumping down in evap2
Thursday, August 18, 2016, 10:14
HS water valves opened...leak detected see attachment for photo from archives
Vented and opened up.
Anders performed leak check, nothing found.
Replaced all seals with blue seals.
Pumping down now
Thursday, August 18, 2016, 16:12
HS water valves opened...leak detected again see attachment for photo of striptool
Vented and opened up.
working with Anders on finding leak...
Monday, August 22, 2016, 10:38
leaks FIXED!
HS water valves opened, NO leaks detected!
Tapped up manually to 70A
Vacuum stable, IGP1 = 2.5e-6 Torr
Initiating auto ramp for TGHT @ 0.2A/min to a max setpoint of 350A
Initiating auto ramp for TBHT @ 0.1A/min to a max setpoint of 230A
Once max setpoints achieved, will tap up manually to final desired temperature of 1900C
Monday, August 22, 2016, 14:58
TGHT = 115A, 1.3V
TBHT = 89A, 0.97V
IGP1 = 4.1e-7 Torr.
Increasing ramping rate to 1.0A/min and 0.5A/min for the TGHT and TBHT respectively.
Monday, August 22, 2016, 16:01
IGP1 = 1.25e-6 torr
TGHT = 174A, 2.2V
TBHT = 118A, 1.4V
Lowering ramping rate to 0.2A/min and 0.1A/min for the TGHT and TBHT respectively for overnight ramping.
|
Tuesday, August 23, 2016, 12:15, John Wong, Empty, 39814-V2-1, LP-IG-LIS, Done, sintering TaC coating on SiC#34 container...round2
|
Laura Lambert wrote: |
Wednesday, August 17, 2016, 17:30
Container coated with TaC using 'flushing technique', cleaned ionizer tube with acetone, so no coating inside ionizer tube
Wrapped with 3 x Ta heat shields, incl center block
Currently pumping down in evap2
Thursday, August 18, 2016, 10:14
HS water valves opened...leak detected see attachment for photo from archives
Vented and opened up.
Anders performed leak check, nothing found.
Replaced all seals with blue seals.
Pumping down now
Thursday, August 18, 2016, 16:12
HS water valves opened...leak detected again see attachment for photo of striptool
Vented and opened up.
working with Anders on finding leak...
Monday, August 22, 2016, 10:38
leaks FIXED!
HS water valves opened, NO leaks detected!
Tapped up manually to 70A
Vacuum stable, IGP1 = 2.5e-6 Torr
Initiating auto ramp for TGHT @ 0.2A/min to a max setpoint of 350A
Initiating auto ramp for TBHT @ 0.1A/min to a max setpoint of 230A
Once max setpoints achieved, will tap up manually to final desired temperature of 1900C
Monday, August 22, 2016, 14:58
TGHT = 115A, 1.3V
TBHT = 89A, 0.97V
IGP1 = 4.1e-7 Torr.
Increasing ramping rate to 1.0A/min and 0.5A/min for the TGHT and TBHT respectively.
Monday, August 22, 2016, 16:01
IGP1 = 1.25e-6 torr
TGHT = 174A, 2.2V
TBHT = 118A, 1.4V
Lowering ramping rate to 0.2A/min and 0.1A/min for the TGHT and TBHT respectively for overnight ramping.
|
Tuesday, August 23, 2016, 12:14
Initiate TGHT autoramping to 400A at 2A/min. Vac 3.5e-7 Torr.
Tuesday, August 23, 2016, 14:48
TGHt tapped up to 420A/7.01V. Local temp read at ~1900C. Will sinter at this temp for a few hours before cooling down.
Tuesday, August 23, 2016, 17:20
TGHT at been at 420A/7.01V for over 4 hours. Vac at 4.8e-7 Torr.
Cooling TGHT and TBHT at 1A/min.
Wednesday, August 24, 2016, 10:35
TGHT/TBHT at 0A.
Venting chamber.
Container looks good.
|
Thursday, August 18, 2016, 10:37, Anders Mjos, , , , Maintenance, New cooling lines for Heat Shield
|
Dan made a set of new cooling lines for the Source Tray Heat Shield cooling yesterday. No joints on the lines. Use same VCR fitting 3/8 -> 1/4" as for the Heat Shield. The old lines had worn threads on the male VCR nut. |
Friday, August 12, 2016, 11:08, Laura Lambert, , , , Maintenance, NEW PUMP FOR GLOVE BOX
|
Wednesday, August 03, 2016, 16:16
Tues July 26th had some problems with the transfer chamber
Transfer chamber was not going below -20in pressure, when usually it will drop all the way to -30in
To by pass and put the uranium target into the glove box, the transfer chamber was flushed 10x - when opened, no change in H2O and O2 in glove box; therefore, 'bypass' worked.
Pump removed and tested by vacuum group - showed no reading on gauge when being tested, how was it even pumping?
New pump installed July 27th.
New pump = bigger/ faster/ quieter
|
Tuesday, August 02, 2016, 13:56, Laura Lambert, SiC, 40860-3, LP-IG-LIS, Done, Sintering SiC#34
|
Tuesday, August 02, 2016, 13:41
Target container contains 471 discs of SiC [6 x 5 packs + 441 single discs]
Target packed length = 16cm.
Mass of SiC(green) = 52.7172g
Container is wrapped with 3 heatshields; no end caps are inserted yet - coated spring inserted both sides to hold discs in place.
Sintering temp = 1800C
TGHT max = 350A. TBHT max at 230A.
Chamber is currently being pumped down.
Slope on OMEGA = 1.04
Tuesday, August 02, 2016, 16:00
Tapped up manually to 30A - vacuum to high, lowered down to 20A to be able to initiate auto-ramp.
IGP1 = 2.3e-5 Torr
Initiating auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
Friday, August 05, 2016, 11:57
Evap2 has reached TGHT = 350A, 5.33V
TBHT = 187A, 2.31V and still climbing...
OMEGA = 1365C
IGP1 = 7.88e-7 Torr
Increased max setpoint for TGHT to 400A.
Friday, August 05, 2016, 13:33
TGHT = 380A, 5.97V
TBHT = 197A, 2.45V
OMEGA = 1396C
IGP1 = 8.75e-7 Torr
Increasing ramping rate to 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
New final setpoint for the TGHT = 450A
Friday, August 05, 2016, 14:17
TBHT = 230A, 2.97V
TGHT = 450A, 7.4V
OMEGA = 1572C
IGP1 = 3.2e-6 Torr
Increasing max setpoint for TGHT to 500A and re-initiating auto-ramp.
Friday, August 05, 2016, 15:18
At TGHT = 480A, OMEGA temperature dropped to 1400C due to coating on window.
Last reading was ~1600C
Tapped up manually to TGHT = 500A, 8.61V
Window fully coated therefore OMEGA reading is negligible at this point
Attempted to take temperature reading with other OMEGA from behind evaporator or using handheld manual temperature reader - all windows have a coating, therefore unsuccessful.
IGP1 = 1.75e-6 Torr
Reduced max voltage set for TGHT to 9.0V to minimize possibly voltage 'creep'
Will remain at these setpoints over wknd and ramp down monday morning.
Monday, August 08, 2016, 08:45
TGHT = 500A on the 'current set' and 466A on the readout, 8.74V
TBHT = 230A, 2.99V
IGP1 = 6.6e-8 Torr
OMEGA = 1460C [reading through coating on window port]
Evap2 has been at these setpoints for the wknd.
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Monday, August 08, 2016, 10:38
Quick observational note:
while ramping down OMEGA readings have slowly increased.
At ~350A OMEGA = ~1500C
At ~300A, OMEGA = ~1750C
Currently at 280A, OMEGA = ~2800C
Coating on window has affected the OMEGA readings in a weird way...
Monday, August 08, 2016, 15:17
Vented in air and opened up this afternoon.
Cleaned windows but left target loaded in evap2 for conditioning process.
|
Tuesday, July 26, 2016, 16:53, Laura Lambert, Ta, 41369-6, HP-SIS, Done, Conditioning Ta#49
|
Tuesday, July 26, 2016, 16:50
loaded into evap2
pumped down, HS water valves opened, no leaks detected.
tapped up manually to 35A
vacuum stable = 3.8e-6 Torr
Initiating auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
Final setpoints at 230A for the TBHT and 600A for the TGHT.
Final desired temperature = 1800C
Wednesday, July 27, 2016, 09:20
IGP1 = 6.3e-7 Torr, vacuum stable.
TGHT = 232A, 2.7V
TBHT = 131A, 1.76V
Increasing ramping rate to 1.0A/min and 0.5A/min for the TGHT and TBHT respectively.
Wednesday, July 27, 2016, 15:46
TGHT = 600A, 8.87V
TBHT = 230A, 3.7V
IGP1 = 1.37e-6 Torr
OMEGA = 1640C
Increased max TGHT voltage to 12V
Tapped up manually to OMEGA = 1810C
TGHT = 675A, 10.21V
IGP1 = 2.2e-6 Torr
Will remain at max setpoints for the rest of the week and cool down over weekend.
Thursday, July 28, 2016, 08:34
TGHT = 675A, 10.41V
OMEGA = 1833C
Tapped down to 660A, 10.09V
OMEGA = 1805C
Friday, July 29, 2016, 13:57
OMEGA = 1814C
TGHT = 660A, 10.16V
TBHT = 230A, 3.72V
IGP1 = 3.43e-7 Torr
evap2 has remained at max setpoints for ~42hrs
conditioning complete.
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Tuesday, August 02, 2016, 13:39
vented in air and removed from evap2 this morning.
target looks good!
|
Friday, July 15, 2016, 11:52, Laura Lambert, Empty, 40860-3, LP-IG-LIS, Done, sintering TaC coating on SiC#34 container
|
Friday, July 15, 2016, 11:49
Container previously coated with TaC using 'flushing technique', cleaned ionizer tube with acetone, so no coating inside ionizer tube
Wrapped with 3 x Ta heat shields, incl center block - new method of each layer being one long single Ta foil covering entire container incl center block
Currently pumping down in evap2
Friday, July 15, 2016, 14:35
Turbo pump broken
Currently being replaced...
Friday, July 15, 2016, 17:04
Turns out its not the turbo pump...TP controls and pump replaced, problem still happening.
Took out heat shield and used a closed loop to rule out leak in chamber, emptied all water lines - turbo pump now on.
Took v.long time to pump down. TP will remain on over wknd.
BP turns on, PV1 turns on, RV turns on - then takes very long time for vacuum to drop ~45min? before BV and TP can be turned on.
Possibly problem with threads on heat shield and not creating proper seal?
Will continue monday with evap2 mystery problem solving...
Monday, July 18, 2016, 16:14
Replaced heat shield and copper seals.
Container re-loaded.
Turbo pump on and good vacuum achieved! YAY!
Finished pumping down, opened HS water valves - no leaks detected.
Tapped up manually to 35A
Vacuum stable, IGP1 = 3e-6 Torr
Initiating auto ramp for TGHT @ 0.2A/min to a max setpoint of 400A
Initiating auto ramp for TBHT @ 0.1A/min to a max setpoint of 230A
Once max setpoints achieved, will tap up manually to final desired temperature of 1900C
Tuesday, July 19, 2016, 09:21
TGHT = 242A, 2.76V
TBHT = 162A
IGP1 = 5.05e-6 Torr
Increasing ramping rate to 1.0A/min and 0.5A/min for the TGHT and TBHT respectively.
Tuesday, July 19, 2016, 13:04
TGHT = 400A, 4.4V
TBHT = 230A, 2.6V
OMEGA = 1120C
Reached max setpoints ~1hr ago.
Tapping up manually to 1900C...
Tuesday, July 19, 2016, 16:32
MORE problems with evap2
TGHT reads 460A, 5.1V, 1170C - a lot of power is being lost somewhere...
Comparison from elog i.d. 291 [the last IGLIS container sintering of TaC coating] the TGHT read 460A, 7.5V, 1900C
Another problem: the read out on the power supply and read out on epics of the TBHT reads 215A; however, the 'current set' says 177A - two very different numbers?!
Ramping down evap2 at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively to further inspect chamber and hopefully solve this...
Wednesday, July 20, 2016, 13:34
Chamber was vented in air and opened up for inspecting.
Fixed!
One of the steel plates used to stop reflection onto the door of the chamber was inserted improperly, resting on top of the 2 negative copper lines to the target leg, this was causing a short.
There was also a short from the right target leg touching the copper heat shield, the heat shield has been shaved down and corrected. It is no longer touching.
There were also 2 brackets that had fallen behind evap2 inside the cage, one was touching the positive lines - it wasn't quite touching the ground, but may have grounded it, causing another possible short.
The chamber was pumped back down and the HS water valves re-opened. No leaks detected.
Evap2 was tapped up manually to 35A.
Vacuum stable = 1.0e-6 Torr.
Initiating auto-ramp at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Final setpoints are TGHT = 400A and TBHT = 230A
Wednesday, July 20, 2016, 16:25
TGHT = 315A, 4.5V
TBHT = 174A, 2.1V
IGP1 = 2e-6 Torr
OMEGA = 1518C
Lowering auto-ramp to 0.2A/min and 0.1A/min for the TGHT and TBHT overnight while unable to keep watch on the vacuum.
Thursday, July 21, 2016, 09:09
Evap 2 reached max setpoints ~7.5hrs ago.
TGHT = 400A, 6.3V
TBHT = 230A, 2.9V
IGP1 = 5.1e-7 Torr.
OMEGA = 1882C
Tapping up manually to 1900C...
Friday, July 22, 2016, 16:18
Container has remained at ~1900C for ~31hrs
TGHT reached 405A/1900C - then after ~23hrs dropped in temperature down to 1895C so was tapped up further to 410A/1910C for another ~8hrs.
TGHT = 410A, 6.57V
IGP1 = 3.1e-7 Torr
TBHT = 230A, 2.9V
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Will remove from evap2 after the weekend.
Tuesday, July 26, 2016, 16:49
vented in air.
container looks good, fully sintered.
will update with photos tomorrow...
|
Monday, June 27, 2016, 11:08, Laura Lambert, Empty, 41790-3, LP-SIS, Done, sintering TaC coating on UCx#17 container
|
Monday, June 27, 2016, 11:07
Container coated with TaC using 'flushing technique'.
Wrapped with 3 x Ta heat shields, incl center block - new method of each layer being one long single Ta foil covering entire container incl center block
Currently pumping down in evap2
Monday, June 27, 2016, 13:23
HS water valves opened
Tapped up manually to 35A
Waited ~1hr, vacuum stable
IGP1 = 1.8e-6 Torr
Initiating auto ramp for TGHT @ 0.2A/min to a max setpoint of 400A
Initiating auto ramp for TBHT @ 0.1A/min to a max setpoint of 230A
Once max setpoints achieved, will tap up manually to final desired temperature of 1900C
Wednesday, June 29, 2016, 11:33
IGP1 = 1.9e-7
TGHT = 400A, 6.0V
TBHT = 223A, 3.9V
OMEGA = 1885C
Remained at these settings for ~13hrs
Increased TBHT max voltage to 4.3V to achieve 230A
TBHT = 230A, 4.1V
OMEGA = 1890C
Tapped up to TGHT = 405A, 6.17V to achieve 1900C...OMEGA reached 1915C
Lowered TGHT to = 403A, 6.12V
OMEGA = 1905C
Measured ~1870C with the mikron, same window the OMEGA measurements are taken out of.
IGP1 = 2.1e-7
Thursday, June 30, 2016, 08:44
TGHT = 403A, 6.07V
OMEGA = 1886C
Tapped back up to 1900C
TGHT = 410A, 6.22V
OMEGA = 1911C
Thursday, June 30, 2016, 16:01
OMEGA = 1911C
Container has remained at ~1900C for ~1.5 days
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Monday, July 04, 2016, 09:59
Vented in air and opened up this morning.
Container looks good.
Confirmed coating fully sintered with J.Wong.
Photos attached.
|
Thursday, June 16, 2016, 11:01, Laura Lambert, SiC, 41369-4, HP-SIS, Done, Conditioning SiC#33 - 1st beta SiC target! 9x
|
Thursday, June 16, 2016, 10:59
Previously sintered over weekend [see elog i.d 306]
Target container contains 450 discs of SiC [4 x 5 packs + 430 single discs]
Target packed length = 16cm.
Mass of 533 discs SiC(green) = 53.8758g
Container is wrapped with 3 heatshields; no end caps are inserted yet - coated spring inserted both sides to hold discs in place.
Conditioning temp = 1800C.
TGHT max = 710A according to sintering data. TBHT max = 230A.
Chamber is currently being pumped down.
Thursday, June 16, 2016, 15:43
Target was not removed from evap2 after sintering, vented and cleaned windows only.
HS water valves already open.
Stepped up manually to 70A, vacuum stable.
Initiated auto-ramp at 1.0A/min for the TGHT and 0.5A/min for the TBHT with max setpoints of 600A and 230A respectively.
TGHT = 118A, 0.9V
TBHT = 90A, 1.1V
IGP1 = 7.3e-7 Torr
Friday, June 17, 2016, 12:14
TGHT has been tapped up manually to reach max desired temperature of 1800C
TGHT = 690A, 10.85V
TBHT = 230A, 3.88V
IGP1 = 4.9e-7 Torr
This is a lower current than the current required to reach 1800C during the sintering process.
For sintering, the max current was determined via extrapolation of trendline from raw data due to interference of coating on window and unable to take reliable readings from OMEGA.
For this conditioning process ~1800C is reached on the OMEGA since the window is still ~un-coated.
Will remain at 690A, ~1800C for several days to maximize conditioning process.
See attachment for raw data.
Monday, June 20, 2016, 09:01
At the end of the day on friday 17th, OMEGA read ~1750C - no change in the current or voltage, vacuum was stable, this was the max setpoints used to reach 1800C.
This morning OMEGA = 2040C
TGHT = 690A, 10.95V
vacuum stable at IGP1 = 1.8e-7 Torr.
Slightly more noticeable coating on window port, looks like a thin ink layer, still relatively thin coating [ see attached image]
Also attached is archive from over wknd to show vacuum stable, current unchanged and voltage negligibly changed [only gone up by ~0.1V]
Friday, June 24, 2016, 13:52
Container has remained at max setpoints for 7 days.
Initiating auto-cool for TGHT @ 2.0A/min and for TBHT @ 1.0A/min.
Will vent chamber and remove from evap2 to pass off for assembly monday morning.
See attachment for updated excel on temperature readings for the conditioning process.
Monday, June 27, 2016, 08:28
vented in air and removed this morning.
target looks good!
all discs remained nicely alligned.
discs expanded outwards ~1cm, pushed back in to keep target length at 16cm
no visible yellow crystals like previous SiC targets
endcaps inserted and expanded.
Rh foil inserted.
Ta heat shield foils removed, fins look good.
see photos attached for pictures of target - post conditioning.
coating on window very hard to remove. looked like a light sharpy pen coating on window. ended up scratching off with acetone and screw driver. couldn't remove all of it... |
Thursday, June 09, 2016, 15:48, Laura Lambert, SiC, 41369-4, HP-SIS, In progress, Sintering SiC#33 - 1st beta-SiC target!
|
Thursday, June 09, 2016, 15:39
First target using beta-SiC material!
Target container contains 450 discs of SiC [4 x 5 packs + 430 single discs]
Target packed length = 16cm.
Mass of 533 discs SiC(green) = 53.8758g
Container is wrapped with 3 heatshields; no end caps are inserted yet - coated spring inserted both sides to hold discs in place.
Sintering temp = 1800C, TGHT will be set accordingly. TBHT max at 230A.
Chamber is currently being pumped down.
Friday, June 10, 2016, 13:24
HS water valves opened, no leaks detected.
Tapping up manually to 70A...
Auto ramp will be set for TGHT = 0.2A/min to a final setpoint of 520A
Auto-ramp for TBHT = 0.1A/min to a final setpoint of 230A.
|
Friday, June 10, 2016, 16:30, John Wong, SiC, 41369-4, HP-SIS, In progress, Sintering SiC#33 - 1st beta-SiC target!
|
Laura Lambert wrote: |
Thursday, June 09, 2016, 15:39
First target using beta-SiC material!
Target container contains 450 discs of SiC [4 x 5 packs + 430 single discs]
Target packed length = 16cm.
Mass of 533 discs SiC(green) = 53.8758g
Container is wrapped with 3 heatshields; no end caps are inserted yet - coated spring inserted both sides to hold discs in place.
Sintering temp = 1800C, TGHT will be set accordingly. TBHT max at 230A.
Chamber is currently being pumped down.
Friday, June 10, 2016, 13:24
HS water valves opened, no leaks detected.
Tapping up manually to 70A...
Auto ramp will be set for TGHT = 0.2A/min to a final setpoint of 520A
Auto-ramp for TBHT = 0.1A/min to a final setpoint of 230A.
|
Friday, June 10, 2016, 16:27
TGHT stepped up to 70A/0.55V. TGHT at 50A/0.62V.
Pressure stabilized at 5.5e-5 Torr.
Initiated auto ramping. TGHT at 0.2A/min --> 520A. TBHT at 0.1A/min --> 230A.
|
Monday, June 13, 2016, 09:53, Laura Lambert, SiC, 41369-4, HP-SIS, In progress, Sintering SiC#33 - 1st beta-SiC target!
|
John Wong wrote: |
Laura Lambert wrote: |
Thursday, June 09, 2016, 15:39
First target using beta-SiC material!
Target container contains 450 discs of SiC [4 x 5 packs + 430 single discs]
Target packed length = 16cm.
Mass of 533 discs SiC(green) = 53.8758g
Container is wrapped with 3 heatshields; no end caps are inserted yet - coated spring inserted both sides to hold discs in place.
Sintering temp = 1800C, TGHT will be set accordingly. TBHT max at 230A.
Chamber is currently being pumped down.
Friday, June 10, 2016, 13:24
HS water valves opened, no leaks detected.
Tapping up manually to 70A...
Auto ramp will be set for TGHT = 0.2A/min to a final setpoint of 520A
Auto-ramp for TBHT = 0.1A/min to a final setpoint of 230A.
|
Friday, June 10, 2016, 16:27
TGHT stepped up to 70A/0.55V. TGHT at 50A/0.62V.
Pressure stabilized at 5.5e-5 Torr.
Initiated auto ramping. TGHT at 0.2A/min --> 520A. TBHT at 0.1A/min --> 230A.
|
Monday, June 13, 2016, 09:51
TGHT = 425A, 5.65V
TBHT = 225A, 3.7V
IGP1 = 8.7e-6 Torr.
Increasing ramping rate to 1.0A/min...
Monday, June 13, 2016, 15:56
Tapped up manually from 520A to 1800C
Extrapolated data on graph to determine correct current required to reach desired max temperature.
Will remain at 1800C for ~48hrs
See attachements for excel sheet and screenshot of striptool.
|
Wednesday, June 15, 2016, 17:58, John Wong, SiC, 41369-4, HP-SIS, In progress, Sintering SiC#33 - 1st beta-SiC target!
|
Laura Lambert wrote: |
John Wong wrote: |
Laura Lambert wrote: |
Thursday, June 09, 2016, 15:39
First target using beta-SiC material!
Target container contains 450 discs of SiC [4 x 5 packs + 430 single discs]
Target packed length = 16cm.
Mass of 533 discs SiC(green) = 53.8758g
Container is wrapped with 3 heatshields; no end caps are inserted yet - coated spring inserted both sides to hold discs in place.
Sintering temp = 1800C, TGHT will be set accordingly. TBHT max at 230A.
Chamber is currently being pumped down.
Friday, June 10, 2016, 13:24
HS water valves opened, no leaks detected.
Tapping up manually to 70A...
Auto ramp will be set for TGHT = 0.2A/min to a final setpoint of 520A
Auto-ramp for TBHT = 0.1A/min to a final setpoint of 230A.
|
Friday, June 10, 2016, 16:27
TGHT stepped up to 70A/0.55V. TGHT at 50A/0.62V.
Pressure stabilized at 5.5e-5 Torr.
Initiated auto ramping. TGHT at 0.2A/min --> 520A. TBHT at 0.1A/min --> 230A.
|
Monday, June 13, 2016, 09:51
TGHT = 425A, 5.65V
TBHT = 225A, 3.7V
IGP1 = 8.7e-6 Torr.
Increasing ramping rate to 1.0A/min...
Monday, June 13, 2016, 15:56
Tapped up manually from 520A to 1800C
Extrapolated data on graph to determine correct current required to reach desired max temperature.
Will remain at 1800C for ~48hrs
See attachements for excel sheet and screenshot of striptool.
|
Wednesday, June 15, 2016, 17:54
TGHT at 710A, 11.35V. TBHT at 230A/3.86V.
Omega reading droppd to 1130C due to coating on windows.
Ionizer tube was measured (center) at around 1900C
Cooling down at 2A/min for TGHT, 1A/min for TBHT.
Samples will be collected prior to cleaning the windows.
NEXT: Conditioning.
|
Thursday, June 16, 2016, 10:58, Laura Lambert, SiC, 41369-4, HP-SIS, Done, Sintering SiC#33 - 1st beta-SiC target!
|
John Wong wrote: |
Laura Lambert wrote: |
John Wong wrote: |
Laura Lambert wrote: |
Thursday, June 09, 2016, 15:39
First target using beta-SiC material!
Target container contains 450 discs of SiC [4 x 5 packs + 430 single discs]
Target packed length = 16cm.
Mass of 533 discs SiC(green) = 53.8758g
Container is wrapped with 3 heatshields; no end caps are inserted yet - coated spring inserted both sides to hold discs in place.
Sintering temp = 1800C, TGHT will be set accordingly. TBHT max at 230A.
Chamber is currently being pumped down.
Friday, June 10, 2016, 13:24
HS water valves opened, no leaks detected.
Tapping up manually to 70A...
Auto ramp will be set for TGHT = 0.2A/min to a final setpoint of 520A
Auto-ramp for TBHT = 0.1A/min to a final setpoint of 230A.
|
Friday, June 10, 2016, 16:27
TGHT stepped up to 70A/0.55V. TGHT at 50A/0.62V.
Pressure stabilized at 5.5e-5 Torr.
Initiated auto ramping. TGHT at 0.2A/min --> 520A. TBHT at 0.1A/min --> 230A.
|
Monday, June 13, 2016, 09:51
TGHT = 425A, 5.65V
TBHT = 225A, 3.7V
IGP1 = 8.7e-6 Torr.
Increasing ramping rate to 1.0A/min...
Monday, June 13, 2016, 15:56
Tapped up manually from 520A to 1800C
Extrapolated data on graph to determine correct current required to reach desired max temperature.
Will remain at 1800C for ~48hrs
See attachements for excel sheet and screenshot of striptool.
|
Wednesday, June 15, 2016, 17:54
TGHT at 710A, 11.35V. TBHT at 230A/3.86V.
Omega reading droppd to 1130C due to coating on windows.
Ionizer tube was measured (center) at around 1900C
Cooling down at 2A/min for TGHT, 1A/min for TBHT.
Samples will be collected prior to cleaning the windows.
NEXT: Conditioning.
|
Thursday, June 16, 2016, 09:29
vented in air and opened up this morning.
took some samples to be tested.
|
Wednesday, May 25, 2016, 11:40, Laura Lambert, Empty, 41369-4, HP-SIS, In progress, sintering TaC coating on SiC#33 container
|
Wednesday, May 25, 2016, 11:37
Container coated with TaC using 'flushing technique' [cleaned ionizer tube with acetone, so no coating inside ionizer tube]
Wrapped with 2 x Ta heat shields - one full height of Ta foil wrapped around cooling fins twice
Currently pumping down in evap2
Thursday, May 26, 2016, 09:28
Tapped up manually to 40A
IGP1 = 6.6e-7 Torr
Initiating auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
Final setpoints for TGHT = 650A and TBHT = 230A
Once max setpoints reached will continue to tap up manually while monitoring temperature to 1900C
|
Tuesday, May 31, 2016, 11:10, John Wong, Empty, 41369-4, HP-SIS, Done, sintering TaC coating on SiC#33 container
|
Laura Lambert wrote: |
Wednesday, May 25, 2016, 11:37
Container coated with TaC using 'flushing technique' [cleaned ionizer tube with acetone, so no coating inside ionizer tube]
Wrapped with 2 x Ta heat shields - one full height of Ta foil wrapped around cooling fins twice
Currently pumping down in evap2
Thursday, May 26, 2016, 09:28
Tapped up manually to 40A
IGP1 = 6.6e-7 Torr
Initiating auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
Final setpoints for TGHT = 650A and TBHT = 230A
Once max setpoints reached will continue to tap up manually while monitoring temperature to 1900C
|
Tuesday, May 31, 2016, 11:09
TGHT at 615A/9.08V, temp = 1610C. Vacuum at 1.8e-7 Torr.
Tapping up TGHT to reach 1900C
Tuesday, May 31, 2016, 12:04
TGHT at 765A/11.90V. Temp at 1900C. Pressure is coming down from 8.7e-7Torr.
Will keep at this temperature for a day.
Wednesday, June 01, 2016, 15:22
Temperature has been stable at 1900C. Pressure is coming down from 3.4e-7 Torr.
Cooling down TGHT and TBHT at 2A/min and 1A/min, respectively.
Friday, June 03, 2016, 12:10
TGHT/TBHT at 0A. Target can be remained under vacuum until Monday.
Monday, June 06, 2016, 16:54
Target container was inspected; it looks good
|
Thursday, May 19, 2016, 14:38, John Wong, SiC, , TARGET BOAT, In progress, Heat-treatment: Beta-SiC (1um) target discs
|
The purpose of this experiment is to determined the limiting operating temperature for Beta-SiC. To do so, samples will be heated in sequence to observe any volatile Si coated on the window. The coating is observed above 1400C for the conventional SiC (mixuture of alpha and beta) and this coating leads to HV shorting problem.
Thursday, May 19, 2016, 14:26
Beta-SiC (size ~1um) slurry was prepared and casted on a graphite foil.
Discs are cut into D-shape
Average thickness (including graphite foil) = 0.349mm
Graphite foil = 0.13mm
Actual SiC thickness = 0.219mm (close to normal SiC thickness)
Samples are loaded into a target boat.
Total discs = 120
Total mass = 14.3507g
Thursday, May 19, 2016, 14:32
Omega slope set to = 1.04
Heat-treatment #1: 1400C
Thursday, May 19, 2016, 17:04
TGHT ramping up to 250A at 0.5A/min
|
Friday, May 20, 2016, 08:54, Laura Lambert, SiC, , TARGET BOAT, In progress, Heat-treatment: Beta-SiC (1um) target discs
|
John Wong wrote: |
The purpose of this experiment is to determined the limiting operating temperature for Beta-SiC. To do so, samples will be heated in sequence to observe any volatile Si coated on the window. The coating is observed above 1400C for the conventional SiC (mixuture of alpha and beta) and this coating leads to HV shorting problem.
Thursday, May 19, 2016, 14:26
Beta-SiC (size ~1um) slurry was prepared and casted on a graphite foil.
Discs are cut into D-shape
Average thickness (including graphite foil) = 0.349mm
Graphite foil = 0.13mm
Actual SiC thickness = 0.219mm (close to normal SiC thickness)
Samples are loaded into a target boat.
Total discs = 120
Total mass = 14.3507g
Thursday, May 19, 2016, 14:32
Omega slope set to = 1.04
Heat-treatment #1: 1400C
Thursday, May 19, 2016, 17:04
TGHT ramping up to 250A at 0.5A/min
|
Friday, May 20, 2016, 08:53
IGP1 = 9.2e-6 Torr.
Increasing ramping rate to 1.0A/min up to 250A
Friday, May 20, 2016, 09:17
IGP1 = 2.1e-5 Torr
TGHT = 215A, 3.1V
OMEGA = 1035C
Stopping auto-ramp and tapping up manually...
Friday, May 20, 2016, 12:26
OMEGA slope changed to 1.04
OMEGA reached ~1430C and kept there for ~1hr.
no change. no coating on window observed
tapped up manually to OMEGA =1500C
TGHT = 350A, 5.8V
Friday, May 20, 2016, 14:17
Not much change to window.
Might be beginning of light dusting, hard to tell.
Will be better observed after longer period of time at 1500C
Will remain at 1500C over weekend.
|
Tuesday, May 24, 2016, 11:18, John Wong, SiC, , TARGET BOAT, In progress, Heat-treatment: Beta-SiC (1um) target discs
|
Laura Lambert wrote: |
John Wong wrote: |
The purpose of this experiment is to determined the limiting operating temperature for Beta-SiC. To do so, samples will be heated in sequence to observe any volatile Si coated on the window. The coating is observed above 1400C for the conventional SiC (mixuture of alpha and beta) and this coating leads to HV shorting problem.
Thursday, May 19, 2016, 14:26
Beta-SiC (size ~1um) slurry was prepared and casted on a graphite foil.
Discs are cut into D-shape
Average thickness (including graphite foil) = 0.349mm
Graphite foil = 0.13mm
Actual SiC thickness = 0.219mm (close to normal SiC thickness)
Samples are loaded into a target boat.
Total discs = 120
Total mass = 14.3507g
Thursday, May 19, 2016, 14:32
Omega slope set to = 1.04
Heat-treatment #1: 1400C
Thursday, May 19, 2016, 17:04
TGHT ramping up to 250A at 0.5A/min
|
Friday, May 20, 2016, 08:53
IGP1 = 9.2e-6 Torr.
Increasing ramping rate to 1.0A/min up to 250A
Friday, May 20, 2016, 09:17
IGP1 = 2.1e-5 Torr
TGHT = 215A, 3.1V
OMEGA = 1035C
Stopping auto-ramp and tapping up manually...
Friday, May 20, 2016, 12:26
OMEGA slope changed to 1.04
OMEGA reached ~1430C and kept there for ~1hr.
no change. no coating on window observed
tapped up manually to OMEGA =1500C
TGHT = 350A, 5.8V
Friday, May 20, 2016, 14:17
Not much change to window.
Might be beginning of light dusting, hard to tell.
Will be better observed after longer period of time at 1500C
Will remain at 1500C over weekend.
|
Tuesday, May 24, 2016, 11:15
Sample has been heated over the long weekend. Temp dropped to 1400C. TGHT at 350A/5.78V. Vac at 1.5e-7 Torr.
It is hard to tell if there is any coating on the window. Will increase temperature to 1800C
Tuesday, May 24, 2016, 11:43
Temp at 1620C. TGHT at 440A/7.7V.
At this temperature, the coating would have been seen for the conventional SiC target material. But, no much of change on the window since the TGHT was tapped up from 1400C.
Continue to increase TGHT to reach 1800C
Tuesday, May 24, 2016, 11:58
Temp at 1680C/TGHT 470A/8.4C - a very light film on the window was observed. Not sure if this film was left from previous processes; it is just that the target container is getting very bright and hard to see.
Tuesday, May 24, 2016, 12:15
TGHT at 510A/9.16V - Observed coating on window. Omega got interfered, therefore temp is unknown. But it was read at ~1720C before the window was getting coated and temp started to dropped.
Will leave at this stage for now...
Tuesday, May 24, 2016, 16:57
Window is fully coated. Based on the heating curve, at 500A, the temp should be at ~1900C (wrapped with a layer of heat shield). Temperature reader dropped to1340C due to the coating interference.
Cooling down TGHT at 2A/min. And will exam the materials tomorrow...
|
Wednesday, May 11, 2016, 17:24, John Wong, np-SiC, , TARGET BOAT, Done, Temperature Treament of Nanofiber SiC/PAN
|
Wednesday, May 11, 2016, 17:15
Nanofiber SiC (~50nm grain size)/PAN was prepared at UBC.
SiC 0.50g, DMF 9.0g, PAN 1.0g, tiny bit of SDS.
The fiber mat was stabilized in air at 250C and then cut into discs, initial mass = 0.1072g
Discs were then bounded with PVA on 9 pieces of rounded graphite foil (green mass gained to 0.6031g)
The stack of naofiber SiC/PAN was loaded on to Ta boated (coated) and wrapped with Ta heat shield.
Chamber is currently being pumped down.
Friday, May 13, 2016, 15:00
TGHT at 390A/6.966V. Temp measured at 1615C.
Will keep at that temperature for a few days.
Monday, May 16, 2016, 15:44
Sample has been heated at ~1600C for 4 days. TGHT at 400A/7.02V.
Cooling down at 2A/min
Tuesday, May 17, 2016, 11:18
Chamber vented. Inspecting samples.
|
Wednesday, May 04, 2016, 13:45, Laura Lambert, , 40282-3, TARGET BOAT, In progress, Conditioning Nb samples for Tobias
|
Wednesday, May 04, 2016, 13:28
Target boat has a layer of niobium foil on the bottom of the boat.
A niobium foil has been made with slots to hold samples [similar to when sintering endcaps] *See attached photos
Larger niobium samples are placed in the slots, holding in place, to avoid warping; smaller niobium sample sitting inside the boat by itself.
Smaller sample closest to OMEGA IR reading [right side]
Boat is wrapped with 1 large layer of Ta foil, wrapped around the boat 3x, careful to avoid touching samples.
Loaded into evap2 yesterday.
Vacuum pump bearings gone - pump replaced this morning by vacuum group.
Pumping down now...
Friday, May 06, 2016, 13:36
HS water valves opened, no leaks detected.
Tapped up manually to 35A.
IGP1 = 2.4e-7 Torr
Setting auto-ramp rate at 0.2A/min to 250A over the weekend.
Will tap up manually monday to final desired temperature of 1400C.
Monday, May 09, 2016, 09:38
OMEGA = 1128C
IGP1 = 1.3e-7 Torr
TGHT = 250A, 3.7V
Tapping up manually to 1400C...
Monday, May 09, 2016, 14:05
Evap2 has reached ~1405C
TGHT = 341A, 5.34V
IGP1 = 1.9e-7 Torr
Will remain at max setpoints for min 4hrs then initiate cool down.
|
Monday, May 09, 2016, 18:19, John Wong, , 40282-3, TARGET BOAT, In progress, Conditioning Nb samples for Tobias
|
Laura Lambert wrote: |
Wednesday, May 04, 2016, 13:28
Target boat has a layer of niobium foil on the bottom of the boat.
A niobium foil has been made with slots to hold samples [similar to when sintering endcaps] *See attached photos
Larger niobium samples are placed in the slots, holding in place, to avoid warping; smaller niobium sample sitting inside the boat by itself.
Smaller sample closest to OMEGA IR reading [right side]
Boat is wrapped with 1 large layer of Ta foil, wrapped around the boat 3x, careful to avoid touching samples.
Loaded into evap2 yesterday.
Vacuum pump bearings gone - pump replaced this morning by vacuum group.
Pumping down now...
Friday, May 06, 2016, 13:36
HS water valves opened, no leaks detected.
Tapped up manually to 35A.
IGP1 = 2.4e-7 Torr
Setting auto-ramp rate at 0.2A/min to 250A over the weekend.
Will tap up manually monday to final desired temperature of 1400C.
Monday, May 09, 2016, 09:38
OMEGA = 1128C
IGP1 = 1.3e-7 Torr
TGHT = 250A, 3.7V
Tapping up manually to 1400C...
Monday, May 09, 2016, 14:05
Evap2 has reached ~1405C
TGHT = 341A, 5.34V
IGP1 = 1.9e-7 Torr
Will remain at max setpoints for min 4hrs then initiate cool down.
|
Monday, May 09, 2016, 18:18
TGHT at 341A/5.34V for over 4 hours. Vac stables at 1.78e-7 Torr.
Cooling down at 2A/min
|
Tuesday, May 10, 2016, 11:57, Laura Lambert, , 40282-3, TARGET BOAT, Done, Conditioning Nb samples for Tobias
|
John Wong wrote: |
Laura Lambert wrote: |
Wednesday, May 04, 2016, 13:28
Target boat has a layer of niobium foil on the bottom of the boat.
A niobium foil has been made with slots to hold samples [similar to when sintering endcaps] *See attached photos
Larger niobium samples are placed in the slots, holding in place, to avoid warping; smaller niobium sample sitting inside the boat by itself.
Smaller sample closest to OMEGA IR reading [right side]
Boat is wrapped with 1 large layer of Ta foil, wrapped around the boat 3x, careful to avoid touching samples.
Loaded into evap2 yesterday.
Vacuum pump bearings gone - pump replaced this morning by vacuum group.
Pumping down now...
Friday, May 06, 2016, 13:36
HS water valves opened, no leaks detected.
Tapped up manually to 35A.
IGP1 = 2.4e-7 Torr
Setting auto-ramp rate at 0.2A/min to 250A over the weekend.
Will tap up manually monday to final desired temperature of 1400C.
Monday, May 09, 2016, 09:38
OMEGA = 1128C
IGP1 = 1.3e-7 Torr
TGHT = 250A, 3.7V
Tapping up manually to 1400C...
Monday, May 09, 2016, 14:05
Evap2 has reached ~1405C
TGHT = 341A, 5.34V
IGP1 = 1.9e-7 Torr
Will remain at max setpoints for min 4hrs then initiate cool down.
|
Monday, May 09, 2016, 18:18
TGHT at 341A/5.34V for over 4 hours. Vac stables at 1.78e-7 Torr.
Cooling down at 2A/min
|
Tuesday, May 10, 2016, 08:45
Vented in air and opened up this morning.
Samples look good!
|
Tuesday, May 03, 2016, 14:44, Laura Lambert, , , , , VACUUM PUMP REPLACEMENT
|
Tuesday, May 03, 2016, 14:29
Turned vacuum pump on this morning, sounded awful: loud grinding bad noises.
Called vacuum group, will replace pump tomorrow morning.
Sounds like materials coming out from all the out-gassing during sintering processes has ruined the bearings.
|
Tuesday, April 26, 2016, 13:50, Laura Lambert, Empty, 40860-2, LP-IG-LIS, Done, sintering TaC coating on UCx#16 container
|
Tuesday, April 26, 2016, 13:32
Container coated with TaC using 'flushing technique'.
Wrapped with 3 x Ta heat shields, incl center block - new method of each layer being one long single Ta foil covering entire container incl center block
Currently pumping down in evap2
Wednesday, April 27, 2016, 10:25
IGP1 = 2.6e-7 Torr.
HS water valves opened, no leaks detected.
Tapped up manually to 35A.
Waited ~35min
Vacuum stable, IGP1 = 6.7e-7 Torr
Initiated auto-ramp at 0.2A/min for the TGHT with a final setpoint of 400A
Final desired temperature = 1900C
Thursday, April 28, 2016, 14:41
Previously TBHT not on when sintering IGLIS container [since no ionizer tube] - John decided will turn on for this round
Tapped up TBHT manually to 140A, 1.69V
IGP1 = 4.5e-7 Torr
OMEGA = 1635C
TGHT = 382A, 5.8V
Initiating auto-ramp of TBHT at 0.1A/min with a final setpoint of 230A.
Friday, April 29, 2016, 08:40
IGP1 = 2.22-7 Torr
TGHT = 400A, 6.1V
TBHT = 233A, 2.9V
OMEGA = 1719C
Tapping up manually to OMEGA = 1900C
Friday, April 29, 2016, 15:22
IGP1 = 3.0e-7 Torr
TGHT = 460A, 7.52V
TBHT =230A, 2.93V
OMEGA = 1904C
Target container has remained at max temperature setpoint of 1900C for 4.5hrs.
Initiating auto cool for TGHT and TBHT at 2.0A/min and 1.0A/min respectively.
Monday, May 02, 2016, 08:35
Vented in air and opened up this morning.
Container looks good.
See attached photos.
|
Sunday, March 13, 2016, 14:58, Aurelia Laxdal, Ta, 41790-1, LP-SIS, In progress, Ta#47 LP-SIS (with new center block) conditioning
|
Started Ta#47 heating at Evap2 using the autoramp program. The TGHT current is setup to go to 300A (for now) and the TBHT to 230A (final value). |
Monday, March 14, 2016, 09:22, Laura Lambert, Ta, 41790-1, LP-SIS, In progress, Ta#47 LP-SIS (with new center block) conditioning
|
Aurelia Laxdal wrote: |
Started Ta#47 heating at Evap2 using the autoramp program. The TGHT current is setup to go to 300A (for now) and the TBHT to 230A (final value).
|
Monday, March 14, 2016, 09:20
One thermocouple was not welded on correctly and is not working.
Cooling evap2 back down, to remove target and re-weld thermocouple.
Once thermocouple replaced, will ramp back up and continue with tests/ conditioning of target.
|
Monday, March 14, 2016, 13:12, Anders Mjos, Ta, 41790-1, LP-SIS, In progress, Ta#47 LP-SIS (with new center block) conditioning
|
Laura Lambert wrote: |
Aurelia Laxdal wrote: |
Started Ta#47 heating at Evap2 using the autoramp program. The TGHT current is setup to go to 300A (for now) and the TBHT to 230A (final value).
|
Monday, March 14, 2016, 09:20
One thermocouple was not welded on correctly and is not working.
Cooling evap2 back down, to remove target and re-weld thermocouple.
Once thermocouple replaced, will ramp back up and continue with tests/ conditioning of target.
|
Monday, March 14, 2016, 13:12: Stopped turbo pump |
Monday, March 14, 2016, 19:22, Aurelia Laxdal, Ta, 41790-1, LP-SIS, In progress, Ta#47 LP-SIS (with new center block) conditioning
|
Anders Mjos wrote: |
Laura Lambert wrote: |
Aurelia Laxdal wrote: |
Started Ta#47 heating at Evap2 using the autoramp program. The TGHT current is setup to go to 300A (for now) and the TBHT to 230A (final value).
|
Monday, March 14, 2016, 09:20
One thermocouple was not welded on correctly and is not working.
Cooling evap2 back down, to remove target and re-weld thermocouple.
Once thermocouple replaced, will ramp back up and continue with tests/ conditioning of target.
|
Monday, March 14, 2016, 13:12: Stopped turbo pump
|
After EVAP2 was vented the thermocouple problem was fixed: it was the wire at on connector inside the box not making proper contact. The lid of the heat shield was also replaced since the one initially mounted had no holes, so one couldn't see the center block. Restarted pumping down at 4:30pm. Just started again the autoramp program: TGHT set to 300A (for the time being) and TBHT to 230A. Temperature measurements will resume tomorrow morning. |
Friday, March 18, 2016, 17:13, Aurelia Laxdal, Ta, 41790-1, LP-SIS, In progress, Ta#47 LP-SIS (with new center block) conditioning
|
Aurelia Laxdal wrote: |
Anders Mjos wrote: |
Laura Lambert wrote: |
Aurelia Laxdal wrote: |
Started Ta#47 heating at Evap2 using the autoramp program. The TGHT current is setup to go to 300A (for now) and the TBHT to 230A (final value).
|
Monday, March 14, 2016, 09:20
One thermocouple was not welded on correctly and is not working.
Cooling evap2 back down, to remove target and re-weld thermocouple.
Once thermocouple replaced, will ramp back up and continue with tests/ conditioning of target.
|
Monday, March 14, 2016, 13:12: Stopped turbo pump
|
After EVAP2 was vented the thermocouple problem was fixed: it was the wire at on connector inside the box not making proper contact. The lid of the heat shield was also replaced since the one initially mounted had no holes, so one couldn't see the center block. Restarted pumping down at 4:30pm. Just started again the autoramp program: TGHT set to 300A (for the time being) and TBHT to 230A. Temperature measurements will resume tomorrow morning.
|
Raised the TGHT at 620A. The TBHT was already set at 230A. The temperature is at 1902 deg C. As per John's instructions the target will condition at these setpoints over the week-end. |
Monday, March 21, 2016, 18:57, Aurelia Laxdal, Ta, 41790-1, LP-SIS, In progress, Ta#47 LP-SIS (with new center block) conditioning
|
Aurelia Laxdal wrote: |
Aurelia Laxdal wrote: |
Anders Mjos wrote: |
Laura Lambert wrote: |
Aurelia Laxdal wrote: |
Started Ta#47 heating at Evap2 using the autoramp program. The TGHT current is setup to go to 300A (for now) and the TBHT to 230A (final value).
|
Monday, March 14, 2016, 09:20
One thermocouple was not welded on correctly and is not working.
Cooling evap2 back down, to remove target and re-weld thermocouple.
Once thermocouple replaced, will ramp back up and continue with tests/ conditioning of target.
|
Monday, March 14, 2016, 13:12: Stopped turbo pump
|
After EVAP2 was vented the thermocouple problem was fixed: it was the wire at on connector inside the box not making proper contact. The lid of the heat shield was also replaced since the one initially mounted had no holes, so one couldn't see the center block. Restarted pumping down at 4:30pm. Just started again the autoramp program: TGHT set to 300A (for the time being) and TBHT to 230A. Temperature measurements will resume tomorrow morning.
|
Raised the TGHT at 620A. The TBHT was already set at 230A. The temperature is at 1902 deg C. As per John's instructions the target will condition at these setpoints over the week-end.
|
Today, lowered the TGHT from 620A (at 1894 deg C) to 300A. TBHT is still at 230A. |
Tuesday, March 22, 2016, 11:31, Aurelia Laxdal, Ta, 41790-1, LP-SIS, In progress, Ta#47 LP-SIS (with new center block) conditioning
|
Aurelia Laxdal wrote: |
Aurelia Laxdal wrote: |
Aurelia Laxdal wrote: |
Anders Mjos wrote: |
Laura Lambert wrote: |
Aurelia Laxdal wrote: |
Started Ta#47 heating at Evap2 using the autoramp program. The TGHT current is setup to go to 300A (for now) and the TBHT to 230A (final value).
|
Monday, March 14, 2016, 09:20
One thermocouple was not welded on correctly and is not working.
Cooling evap2 back down, to remove target and re-weld thermocouple.
Once thermocouple replaced, will ramp back up and continue with tests/ conditioning of target.
|
Monday, March 14, 2016, 13:12: Stopped turbo pump
|
After EVAP2 was vented the thermocouple problem was fixed: it was the wire at on connector inside the box not making proper contact. The lid of the heat shield was also replaced since the one initially mounted had no holes, so one couldn't see the center block. Restarted pumping down at 4:30pm. Just started again the autoramp program: TGHT set to 300A (for the time being) and TBHT to 230A. Temperature measurements will resume tomorrow morning.
|
Raised the TGHT at 620A. The TBHT was already set at 230A. The temperature is at 1902 deg C. As per John's instructions the target will condition at these setpoints over the week-end.
|
Today, lowered the TGHT from 620A (at 1894 deg C) to 300A. TBHT is still at 230A.
|
Cooling down the target.
|
Thursday, March 24, 2016, 11:32, John Wong, Ta, 41790-1, LP-SIS, Done, Ta#47 LP-SIS (with new center block) conditioning
|
Aurelia Laxdal wrote: |
Aurelia Laxdal wrote: |
Aurelia Laxdal wrote: |
Aurelia Laxdal wrote: |
Anders Mjos wrote: |
Laura Lambert wrote: |
Aurelia Laxdal wrote: |
Started Ta#47 heating at Evap2 using the autoramp program. The TGHT current is setup to go to 300A (for now) and the TBHT to 230A (final value).
|
Monday, March 14, 2016, 09:20
One thermocouple was not welded on correctly and is not working.
Cooling evap2 back down, to remove target and re-weld thermocouple.
Once thermocouple replaced, will ramp back up and continue with tests/ conditioning of target.
|
Monday, March 14, 2016, 13:12: Stopped turbo pump
|
After EVAP2 was vented the thermocouple problem was fixed: it was the wire at on connector inside the box not making proper contact. The lid of the heat shield was also replaced since the one initially mounted had no holes, so one couldn't see the center block. Restarted pumping down at 4:30pm. Just started again the autoramp program: TGHT set to 300A (for the time being) and TBHT to 230A. Temperature measurements will resume tomorrow morning.
|
Raised the TGHT at 620A. The TBHT was already set at 230A. The temperature is at 1902 deg C. As per John's instructions the target will condition at these setpoints over the week-end.
|
Today, lowered the TGHT from 620A (at 1894 deg C) to 300A. TBHT is still at 230A.
|
Cooling down the target.
|
Thursday, March 24, 2016, 11:29
Target was removed from the Evaporator.
The thermocouples broke off.
Need to insert Re foil prior to installing
|
Tuesday, April 19, 2016, 09:28, Anders Mjos, Ta, 41790-1, LP-SIS, Done, Ta#47 LP-SIS (with new center block) conditioning
|
John Wong wrote: |
Aurelia Laxdal wrote: |
Aurelia Laxdal wrote: |
Aurelia Laxdal wrote: |
Aurelia Laxdal wrote: |
Anders Mjos wrote: |
Laura Lambert wrote: |
Aurelia Laxdal wrote: |
Started Ta#47 heating at Evap2 using the autoramp program. The TGHT current is setup to go to 300A (for now) and the TBHT to 230A (final value).
|
Monday, March 14, 2016, 09:20
One thermocouple was not welded on correctly and is not working.
Cooling evap2 back down, to remove target and re-weld thermocouple.
Once thermocouple replaced, will ramp back up and continue with tests/ conditioning of target.
|
Monday, March 14, 2016, 13:12: Stopped turbo pump
|
After EVAP2 was vented the thermocouple problem was fixed: it was the wire at on connector inside the box not making proper contact. The lid of the heat shield was also replaced since the one initially mounted had no holes, so one couldn't see the center block. Restarted pumping down at 4:30pm. Just started again the autoramp program: TGHT set to 300A (for the time being) and TBHT to 230A. Temperature measurements will resume tomorrow morning.
|
Raised the TGHT at 620A. The TBHT was already set at 230A. The temperature is at 1902 deg C. As per John's instructions the target will condition at these setpoints over the week-end.
|
Today, lowered the TGHT from 620A (at 1894 deg C) to 300A. TBHT is still at 230A.
|
Cooling down the target.
|
Thursday, March 24, 2016, 11:29
Target was removed from the Evaporator.
The thermocouples broke off.
Need to insert Re foil prior to installing
|
Tuesday, April 19, 2016, 09:28: Uploaded thermoucouple data. |
Thursday, April 07, 2016, 15:23, John Wong, SiC, , TARGET BOAT, Done, E-spun SiC/PAN thermal treatment
|
Thursday, April 07, 2016, 15:18
E-spun SiC/PAN fiber mats were produced at UBC.
12%PAN solution; 50% SiC to weight of PAN.
Materials used:
1.2g PAN, 8.8g DMF, 0.6g SiC, SDS ~0.1% to SiC
Fiber mats were heat treated at 250C in air. Then cut into 18" discs and loaded into Ta target boat with heatshield wrapped.
3 temperature treatments will carry out: 1200C, 1400C and 1600C
Chamber is being pumped down
Friday, April 08, 2016, 10:02
TGHT at 285A, Temp at ~1200C. Will remain at this temp for a few hours before cooling down.
Some samples will be taken out for analysis.
Next week, temperature treatment will continue at 1400C
Friday, April 08, 2016, 14:26
Samples have been heated at 1200C for just over 4 hours.
Initiated auto-cooling at 2A/min
Tuesday, April 12, 2016, 17:51
Heat treatment #2 - 1400C.
Initial mass after 1200C = 0.0312g
Monday, April 18, 2016, 12:55
Samples was heated at 1400C (TGHT maintained at ~370A) for 4 days (see attachment 1).
Chamber is vented; samples will be inspected.
Tuesday, April 19, 2016, 17:49
Results
Sample mass after 1200C = 0.0312g
Sample mass after 1400C = 0.0294g
~5.78% mass loss.
Tuesday, April 19, 2016, 17:57
Heat Treatment#3: 1600C
sample mass before heating = 0.0238g (this sample is taken from the batch after it was heated at 1400C)
Chamber is being pumped.
Thursday, April 21, 2016, 11:07
TGHT stepped up to 330A, temp measured at 1422C.
Thursday, April 21, 2016, 12:05
TGHT at 415A/7.16V; temp at 1610C
Thursday, April 21, 2016, 17:49
Temp dropped to 1590. Increased TGHT to 425A; temp reads 1602A.
Friday, April 22, 2016, 10:57
Voltage increased to 7.33V, TGHT stepped down to 418A, temp maintained at 1610A.
Monday, April 25, 2016, 12:08
Sample was heat treated for almost 4 days. Temperature dropped to 1578C, TGHT at 418/7.26V. (see attachment #2)
Ramping down TGHT 2A/min.
Monday, April 25, 2016, 16:00
Result:
Mass after 1600C = 0.0104g, 5.63% mass loss.
Will do XRD/EDX
|
Wednesday, March 30, 2016, 11:32, John Wong, , Target boat, TARGET BOAT, Done, Thermostablization Polycarbosilane Fibers (UBC MTRL Samples)
|
Wednesday, March 30, 2016, 11:30
Polycarbosilane fibers were prepared by UBC MTRL.
Two samples with different fiber sizes were loaded in target boat and wrapped with heat shields.
Samples will be heated up to 1600C.
Chamber is currently being pumped down
Thursday, March 31, 2016, 16:49
Ramping up TGHT to 300A at 1A/min
Tuesday, April 05, 2016, 13:02
Samples was heated at 1600C for about 3 hours.
Then it was cooled down at 2A/min.
The process is complete.
|
Thursday, March 24, 2016, 12:05, John Wong, SiC, , TARGET BOAT, Done, Test#3: E-spin SiC with PAN
|
Thursday, March 24, 2016, 11:37
SiC powder (<1um) [10%] was mixed with PAN solution [10%]. Solution was sonicated before e-spinning.
Fiber mat was binded to graphite foil and heat treated to 250C in air for 1 hour.
Samples were cut in pieces and rolled up and inserted in Ta target container (TaC coated). Heat shield was added.
Heat Treatment #1:
Temperature: 1600C (~350A)
Ramping up TGHT to 300A at 1A/min.
Tuesday, March 29, 2016, 11:11
TGHT was maintained at 410A for 1600C for 2 days (see attachment 1). However at around 22:30 on March 28, there was a sudden increase in voltage.
Temperature raised up to 1750C. Not sure there was a fault with the control system and it was caused by the Ta-heat shield. (see attachment #2).
Target was cooled down around 2am on March 29.
Samples will be removed from the chamber.
|
Friday, February 26, 2016, 16:02, John Wong, np-SiC, , TARGET BOAT, Done, Test#2: Carbonizing sol-gel TEOS + Pan nanofibers
|
Friday, February 26, 2016, 15:44
5 samples were prepared at UBC MTRL using Sol-gel tetraethyl orthosilicate (TEOS) coated on electrospun polyacrylonitrate (PAN).
Each sample is sandwiched in between graphite foils.
Sample labeling:
Direct, 0.2358g
Mix, 0.3486g
3X, 0.2273g
5x, 0.2079g
7x, 0.1735g
All samples are loaded in the target boat, stacking on each other. The Container is wrapped with 2X- Ta shields.
Chamber is pumping down.
Step#1 Carbonization temperature: 1600C
Saturday, February 27, 2016, 10:07
Vac at 2.5e-7 torr.
Ramping up TGHT to 300A at 1A/min. monitoring temp.
Saturday, February 27, 2016, 17:38
TGHT at 400A, temp at 1600C. Vac 1.34e-6 Torr.
Monday, February 29, 2016, 13:04
Samples have been heated at 1635C for almost 2 days.
Pressure at 2.1e-7 Torr.
Initiated cooling at 2A/min.
Thursday, March 24, 2016, 11:26
Samples were analyzed for Si using EDX. Unfortunately, no Si was found. The vapour pressure of SiO was too high for it to react with PAN to carbonize in a vacuum environment.
Will look into a different technique.
|
Wednesday, February 24, 2016, 17:40, John Wong, Nb, , LP-SIS, Done, Bob/Tobi Nb samples
|
Thursday, February 25, 2016, 18:04 Wednesday, February 24, 2016, 17:29
Heat treatment of 2 bullet-shaped Nb samples in a LP-SIS container; it is just that we don't have a target boat.
Container is wrapped with 12" in total length. A strip of Nb foil is used as an underlayer for the samples to sit on top.
Chamber has been pumped down and current vacuum at 1e-6 Torr.
HS water check - good.
Target temperature 1400C
Ramping up to 250A; this should get to ~1300C. Will let it heat for over night and step up to 1400C tomorrow.
Wednesday, February 24, 2016, 17:59
I'm stopping the heating process because the camera is not working. I can't monitor the temperature. Tried to fit the camera; don't now why it fails to connect to the server.
Will look in to it tomorrow...
Thursday, February 25, 2016, 08:17
Initiated auto ramping TGHT at 2A/min.
Thursday, February 25, 2016, 17:33
Finally the camera is fixed.
Current temperature is at 1126C, TGHT at 250A. Will step up to reach 1400C.
Thursday, February 25, 2016, 18:04
TGHT stepped up to 335A to reach 1400C. (see attachment)
Will heat this for few hours and cool it at around 11pm tonight.
Thursday, February 25, 2016, 22:19
Samples have been heated over 4.5 hours.
Initiated cool down at 1A/min.
Friday, February 26, 2016, 15:43
done! all good.
|
Tuesday, February 16, 2016, 14:02, Laura Lambert, Empty, 40202-5, TARGET BOAT, In progress, sintered TaC coating on target boat [container style with no ionizer tube]
|
Tuesday, February 16, 2016, 14:19
coated with TaC yesterday and let dry overnight.
wrapped with one long Ta heat shield - wrapped around tube 3x, with Ta wire to offset Ta foil away from container
loaded into evap2 and currently pumping down.
Wednesday, February 17, 2016, 10:51
HS water valves opened, no leaks detected.
Tapped up manually to 35A.
Waited ~20min, vacuum stable.
IGP1 = 5.9e-7 Torr.
Initiating auto-ramp at 0.2A/min to a final setpoint of 400A.
Final desired temperature = 1900C
Thursday, February 18, 2016, 09:16
IGP1 = 6.6e-7 Torr.
TGHT = 303A, 4.3V
OMEGA = 1311C
Increasing ramping rate to 1.0A/min.
|
Thursday, February 18, 2016, 13:22, John Wong, Empty, 40202-5, TARGET BOAT, In progress, sintered TaC coating on target boat [container style with no ionizer tube]
|
Laura Lambert wrote: |
Tuesday, February 16, 2016, 14:19
coated with TaC yesterday and let dry overnight.
wrapped with one long Ta heat shield - wrapped around tube 3x, with Ta wire to offset Ta foil away from container
loaded into evap2 and currently pumping down.
Wednesday, February 17, 2016, 10:51
HS water valves opened, no leaks detected.
Tapped up manually to 35A.
Waited ~20min, vacuum stable.
IGP1 = 5.9e-7 Torr.
Initiating auto-ramp at 0.2A/min to a final setpoint of 400A.
Final desired temperature = 1900C
Thursday, February 18, 2016, 09:16
IGP1 = 6.6e-7 Torr.
TGHT = 303A, 4.3V
OMEGA = 1311C
Increasing ramping rate to 1.0A/min.
|
Thursday, February 18, 2016, 13:10
TGHT reached to 450A, temp at 1800C. Stepped up TGHT 490A, temp measured at ~1900C.
|
Thursday, February 18, 2016, 17:21, Laura Lambert, Empty, 40202-5, TARGET BOAT, Done, sintered TaC coating on target boat [container style with no ionizer tube]
|
John Wong wrote: |
Laura Lambert wrote: |
Tuesday, February 16, 2016, 14:19
coated with TaC yesterday and let dry overnight.
wrapped with one long Ta heat shield - wrapped around tube 3x, with Ta wire to offset Ta foil away from container
loaded into evap2 and currently pumping down.
Wednesday, February 17, 2016, 10:51
HS water valves opened, no leaks detected.
Tapped up manually to 35A.
Waited ~20min, vacuum stable.
IGP1 = 5.9e-7 Torr.
Initiating auto-ramp at 0.2A/min to a final setpoint of 400A.
Final desired temperature = 1900C
Thursday, February 18, 2016, 09:16
IGP1 = 6.6e-7 Torr.
TGHT = 303A, 4.3V
OMEGA = 1311C
Increasing ramping rate to 1.0A/min.
|
Thursday, February 18, 2016, 13:10
TGHT reached to 450A, temp at 1800C. Stepped up TGHT 490A, temp measured at ~1900C.
|
Thursday, February 18, 2016, 17:21
TGHT remained at max setpoint for 4hrs.
IGP1 = 6.6e-7 Torr.
OMEGA = 1913C
Initiating auto-cool for TGHT at 2.0A/min.
Friday, February 19, 2016, 14:17
evap2 vented and opened up this morning.
container looks good.
|
Friday, February 12, 2016, 11:09, Laura Lambert, Empty, 41077-1, LP-SIS, Done, sintering TaC coated small center block container
|
Friday, February 12, 2016, 11:01
Container coated with TaC with new method - ends tapped off, liquid poured/swirled around container, then poured back out - 'flushing technique'.
Container wrapped with 3 x Ta heat shields, incl center block - new method of each layer being one long single Ta foil covering entire container incl center block
IGP1 = 6.3e-7Torr
HS water valves opened, no leaks detected.
Tapped up manually to 35A.
Waited ~20min.
Vacuum stable, IGP1 = 1.3e-6 Torr.
Initiated auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively with final setpoints of 400A and 230A.
Monday, February 15, 2016, 08:56
IGP1 = 3.9e-7 Torr.
TBHT = 230A, 4.0V
TGHT = 400A, 6.58V
OMEGA = 1766C
Tapping up manually to 1900C...
Monday, February 15, 2016, 10:18
IGP1 = 5e-7 Torr
TGHT = 450A, 7.55V
OMEGA = 1913C
Monday, February 15, 2016, 14:30
IGP1 = 4.9e-7 Torr.
TGHT = 450A, 7.55V.
Material remained at ~1910C for ~4hrs.
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Tuesday, February 16, 2016, 14:17
vented in air and opened up this morning.
target container sintered nicely.
|
Tuesday, January 19, 2016, 14:27, John Wong, np-SiC, targetboat (TaC coated), TARGET BOAT, Done, SiC Nanofiber Heat Treatment
|
Tuesday, January 19, 2016, 14:19
SiC nanofiber was prepared at UBC Material Engineering Sci.
4 samples are loaded in a Ta target contained (sintered with TaC coating):
Sample 1:
size: 21.70 x 21.54 mm, mass: 0.0762g, thick: 0.224mm
Sample 2:
size: 20.89mm x 23.95mm, mass: 0.0954g, thick: 0.232mm
--> Sample 1 and 2 with graphite backing foil
Sample 3:
size: 22.55 x 25.56mm, mass: 0.0082g, thick: 0.110mm
Sample 4: 16.93 x 23.82mm, mass: 0.0048g, thick: 0.086mm
--> Sample 3 and 4 with no graphite backing foil.
(see attachment)
Test#1: Heating temperature at 1600C for 24hrs.
TGHT will be adjusted accordingly. There are 2 Ta-heat shields wrapped around the container.
Chamber is currently being pumped down.
Tuesday, January 19, 2016, 16:19
Vacuum at 2.0e-6 Torr.
For 1600C, expected current is around 350A.
Stepping up TGHT gradually...
Wednesday, January 20, 2016, 14:34
TGHT was ramped up to 390A/6.63V to reach 1600C. Samples have been heated at that temp since 11pm last night.
Visual check on the fibers seem ok (see attachment).
Will continue to heat this for a total time of 24hours.
Wednesday, January 20, 2016, 22:57
Samples have been heated at 1600C for 24hours.
Initiated cooling at 1A/min.
Wednesday, January 27, 2016, 12:34
First attempt - heating 1600C. XRD result showed board "bumps" that could be SiO2? It is inconclusive.
Second attempt - re-heating the same samples, namely
Sample 1 - only the fiber
Sample 2 - with graphite backing. This sample is loaded with the fiber facing down to see how well it holds on the graphite foil. (see attachment)
TGHT will be ramped up to reach 1800C
Chamber is currently being pumped down.
Wednesday, January 27, 2016, 14:04
Water valves open; no leaks detected.
Ramping up TGHT to 400A at 2A/min
Wednesday, January 27, 2016, 18:08
TGHT is at 481A to obtain 1800C.
Visual check on Sample 2 - fiber has fallen off graphite backing foil.
Will remain heated at this temperature for over night.
Friday, February 12, 2016, 11:11
Heat treatment test#1 is complete. XRD results are inconclusive. Need to do EDX to determine Si/SiO2.
(See my dropbox for more details)
|
Thursday, January 14, 2016, 11:48, Laura Lambert, , , , Maintenance, Backing Pump Replaced
|
Thursday, January 14, 2016, 11:47
Backing pump was making very loud high pitched noises during last couple processes in the evaporator.
Replaced with a new one this morning.
|
Monday, January 11, 2016, 15:47, Laura Lambert, SiC, 41077-3, LP-SIS, Done, Conditioning SiC test target for test stand measurements
|
Monday, January 11, 2016, 15:25
Small center block LP-SIS container previously sintered with TaC coating
3x Ta heat shields
Container is loaded with 260 discs of SiC with a total length of 8.5cm
Loaded into evap2 and pumped down this morning
HS water valves opened up, no leaks detected
Tapped up manually to 30A
Vacuum stable
IGP1 = 1e-6 Torr
Initiating auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively
Final setpoints: 400A for the TGHT and 230A for the TBHT
Final desired temperature: 1700C
Tuesday, January 12, 2016, 12:55
TGHT = 138A, TBHT = 80A
IGP1 = 7.7e-6 Torr.
Vacuum stable and coming down.
Increasing ramping rate to 0.5A/min and 0.2A/min for the TGHT and TBHT respectively.
Wednesday, January 13, 2016, 09:32
TGHT reached 400A ~11.5hrs ago
TBHT reached 230A ~8hrs ago
OMEGA = 1400C
IGP1 = 1.75e-7 Torr
Tapping up manually to 1700C...
Wednesday, January 13, 2016, 10:14
Previous temperature measurement of OMEGA = 1400C is wrong due to window port being coated with SiC [see attached photos]
Will remain at TGHT = 420A for 4hrs then cool down this afternoon
Wednesday, January 13, 2016, 14:29
Remained at max setpoints for 4.5hrs.
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Thursday, January 14, 2016, 09:47
Vented in air and opened up this morning
Target looks good
Will insert and expand endcaps this afternoon
|
Thursday, January 07, 2016, 09:19, Aurelia Laxdal, Ta, 41369-5, HP-SIS, In progress, Temperature measurements
|
Temperature measurements in progress this week for Ta HP-SIS.
See attachment for the current settings and rampings of the TGHT/TBHT for the temperature measurements taken on Jan. 9-10, 2016 .
Note: TBHT PS tripped off on Jan. 9, 2016 (see first page of the attached file) and couldn't turn it ON again over the week-end. |
Friday, January 08, 2016, 11:15, Laura Lambert, Ta, 41369-5, HP-SIS, Done, Temperature measurements
|
Aurelia Laxdal wrote: |
Temperature measurements in progress this week for Ta HP-SIS.
|
Friday, January 08, 2016, 10:49
Rh foil added.
endcaps inserted and expanded.
total length of target with end caps = 3.45cm
spot weld one thermocouple onto center block and one thermocouple onto target leg [left side wrt ionizer tube into page].
see elog id# 268 for more info regarding measurements taken and state of TBHT power supply...
|
Wednesday, December 16, 2015, 10:22, Laura Lambert, Ta, 41369-5, HP-SIS, Done, Conditioning back-up Ta Target & emissivity measurements
|
Wednesday, December 16, 2015, 10:09
Target consists of 505 discs.
Total packed length 3.4cm.
*same parameters at Ta#46*
Total mass of target materials 53.9381g [4 packs of 20 with Ta wire + 425 single discs].
3 x Ta Heat shields.
No Re foil inserted.
No endcaps inserted.
Chamber pumped down overnight.
IGP1 = 5.1e-7 Torr.
Tapped up manually to 35A.
IGP1 = 5.2e-7 Torr.
Vacuum stable, initiating auto-ramp.
TBHT will be ramped up to 230A at 1.0A/min.
TGHT will be ramped up to 1800C, auto ramp to 600A at 2.0A/min [estimated final value of 720A according to elog ID 239]
Wednesday, December 16, 2015, 15:08
TBHT reached max setpoint of 230A, 3.3V
TGHT = 600A, 8.9V
IGP1 = 1.1e-6 Torr.
OMEGA = 1543C
Increasing final setpoint of TGHT to 700A and re-initiating auto-ramp.
Wednesday, December 16, 2015, 16:02
TGHT = 700A, 10.6V
IGP1 = 2.1e-6 Torr.
OMEGA = 1740C
Tapping up manually to 1800C.
Wednesday, December 16, 2015, 16:28
TGHT = 730A, 11.2V
Vacuum is coming down from IGP1 = 2.6e-6 Torr.
OMEGA = 1800C
Will condition the target at 1800C overnight and ramp down in the morning.
Thursday, December 17, 2015, 09:31
OMEGA = 1802C on right side
Temp on leg of left side = 2150C, the hottest point - measured with the Mikron pyrometer.
Friday, December 18, 2015, 08:53
Evap2 remained at 1800C for ~26.5hrs
Auto-ramped down to TGHT = 300A and TBHT = 90A at a rate of 2.0A/min and 1.0A/min respectively.
Conditioning complete.
TGHT will be ramped up later today for emissivity measurements.
Monday, January 04, 2016, 11:21
the following was performed by aurelia.
emissivity measurements were taken late december.
evap2 was cooled down and left under vacuum over the xmas break.
currently ramping back up for more emissivity measurements.
Friday, January 08, 2016, 10:47
Aurelia done measurements.
vented and opened this morning.
|
Monday, December 07, 2015, 09:06, Laura Lambert, Empty, 39530-9, HP-FEBIAD, Done, emissivity measurements with no h.s on HP-FEBIAD container - round2
|
Monday, December 07, 2015, 09:04
No heat shields.
Container empty.
IGP1 = 1.1e-7 Torr.
Slope of OMEGA = 0.98
Tapped up manually to 35A.
Vacuum stable, initiating auto-ramp at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Final setpoints: TBHT = 90A, TGHT = 360A
Will tap up with the same parameters as last round to confirm results.
Friday, December 11, 2015, 11:44
Took out of evap2 yesterday.
Aurelia took many emissivity measurements to compare with previous data - which matched up.
The dip in emissivity before going up again around ~560A could be due to oxidation of the materials.
|
Thursday, September 24, 2015, 09:48, Laura Lambert, Empty, 41077-5, , In progress, Sintering TaC coating container for UCx Target
|
Thursday, September 24, 2015, 08:39
IGP1 = 6.5e-7Torr
HS water valves opened, no leaks detected.
Tapped up manually to 35A.
Waited ~20min.
Vacuum stable, IGP1 = 1.5e-6 Torr.
Initiated auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively with final setpoints of 250A and 230A.
Final temp of 1200C on auto-ramp in order to initiate temperature measurements starting at ~1200C.
Thursday, September 24, 2015, 10:24
IGP1 = 8.7e-7 Torr
TGHT = 44A, TBHT = 38A
Increasing auto-ramp to 0.5A/min and 0.2A/min for the TGHT and TBHT respectively.
Thursday, September 24, 2015, 12:03
Vacuum spiking rapidly.
Stopped auto-ramp, tapped TGHT and TBHT down manually, allowing vacuum to stabilize.
IGP1 = 3.5e-6 Torr.
Re-initiating auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
|
Thursday, September 24, 2015, 12:18, John Wong, Empty, 41077-5, LP-SIS, Done, Sintering TaC coating container for UCx Target
|
Laura Lambert wrote: |
Thursday, September 24, 2015, 08:39
IGP1 = 6.5e-7Torr
HS water valves opened, no leaks detected.
Tapped up manually to 35A.
Waited ~20min.
Vacuum stable, IGP1 = 1.5e-6 Torr.
Initiated auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively with final setpoints of 250A and 230A.
Final temp of 1200C on auto-ramp in order to initiate temperature measurements starting at ~1200C.
Thursday, September 24, 2015, 10:24
IGP1 = 8.7e-7 Torr
TGHT = 44A, TBHT = 38A
Increasing auto-ramp to 0.5A/min and 0.2A/min for the TGHT and TBHT respectively.
|
Thursday, September 24, 2015, 12:04
A few notes about the target container:The Ta-foil is cut in a full length of the target container, and that also covers up the back block, and the container is wrapped with 3 sheets (see attachment)
The inner tube is coated with TaC, using the "flushing technique" - the coating looks much better; will see how it turns out after the sintering process
The target will be heated up to 1900C . Due to the new wrapping of the Ta-heat shield, the heat distribution may be different. So the target heater will be ramped up to achieve the desired temperature.
Thursday, September 24, 2015, 18:45
TGHT reached to 250A3.6V, TGHT at 230A and stayed for 1.5 hours. Temp-L = 1280C, Temp-R = 1360C.
Auto-ramp TGHT to 500A at 1A/min and heat at that current for overnight. Will take temp reading tomorrow.
Thursday, September 24, 2015, 23:08
TGHT has reached to 500A/8.57V. Temp-L = 1895C, Temp-R = 2073C. (Not sure why the temperature is real, will need to investigate more to get an absolute temp)
Just to be safe… Ramping down TGHT to 425A (according to e-log id 216, Temp-R reached to 1800C with TGHT at 425A/6.84V, but no temp measured for the left at that time)
Will check again later.
Friday, September 25, 2015, 11:52
The target has been heated at 420A for ~12hours; temp measured ~1900C, slightly higher than the previous target container (W.O#40860-1); the Ta-wraping could affect the heat distribution.
The temperature is also confirmed by using the 2-C digital pyrometer. The tube inner surface is measured about 1900C, and the ionizer tube is about 2400C. (see attachment #2).
Initiating auto-cooling at 2A/min for TGHT and 1A/min for TBHT.
The target will be inspected next Monday
Wednesday, September 30, 2015, 16:01
The target container is fully sintered (see attachment#3)
It is still in the discussion where this container will be used online for the UCx. Nevertheless, the target contain is ready and it looks pretty good.
|
Tuesday, October 06, 2015, 15:18, John Wong, Empty, 41077-5, LP-SIS, In progress, Test#1: Measuring temp with thermocouple (centre) & 2C-IR
|
John Wong wrote: |
Laura Lambert wrote: |
Thursday, September 24, 2015, 08:39
IGP1 = 6.5e-7Torr
HS water valves opened, no leaks detected.
Tapped up manually to 35A.
Waited ~20min.
Vacuum stable, IGP1 = 1.5e-6 Torr.
Initiated auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively with final setpoints of 250A and 230A.
Final temp of 1200C on auto-ramp in order to initiate temperature measurements starting at ~1200C.
Thursday, September 24, 2015, 10:24
IGP1 = 8.7e-7 Torr
TGHT = 44A, TBHT = 38A
Increasing auto-ramp to 0.5A/min and 0.2A/min for the TGHT and TBHT respectively.
|
Thursday, September 24, 2015, 12:04
A few notes about the target container:The Ta-foil is cut in a full length of the target container, and that also covers up the back block, and the container is wrapped with 3 sheets (see attachment)
The inner tube is coated with TaC, using the "flushing technique" - the coating looks much better; will see how it turns out after the sintering process
The target will be heated up to 1900C . Due to the new wrapping of the Ta-heat shield, the heat distribution may be different. So the target heater will be ramped up to achieve the desired temperature.
Thursday, September 24, 2015, 18:45
TGHT reached to 250A3.6V, TGHT at 230A and stayed for 1.5 hours. Temp-L = 1280C, Temp-R = 1360C.
Auto-ramp TGHT to 500A at 1A/min and heat at that current for overnight. Will take temp reading tomorrow.
Thursday, September 24, 2015, 23:08
TGHT has reached to 500A/8.57V. Temp-L = 1895C, Temp-R = 2073C. (Not sure why the temperature is real, will need to investigate more to get an absolute temp)
Just to be safe… Ramping down TGHT to 425A (according to e-log id 216, Temp-R reached to 1800C with TGHT at 425A/6.84V, but no temp measured for the left at that time)
Will check again later.
Friday, September 25, 2015, 11:52
The target has been heated at 420A for ~12hours; temp measured ~1900C, slightly higher than the previous target container (W.O#40860-1); the Ta-wraping could affect the heat distribution.
The temperature is also confirmed by using the 2-C digital pyrometer. The tube inner surface is measured about 1900C, and the ionizer tube is about 2400C. (see attachment #2).
Initiating auto-cooling at 2A/min for TGHT and 1A/min for TBHT.
The target will be inspected next Monday
Wednesday, September 30, 2015, 16:01
The target container is fully sintered (see attachment#3)
It is still in the discussion where this container will be used online for the UCx. Nevertheless, the target contain is ready and it looks pretty good.
|
Tuesday, October 06, 2015, 15:09
After further discussion, we are going to reheat this container to 420A. The temperature will be measured with the thermocouple - probe inside the centre of the tube - and the 2C-IR for comparison.
This test is to ensure that the container is actually heated to 1900C before the UCx material can be loaded
The chamber has been pumped down to 1.92e-6 Torr. Heat shield valve is open and no leaks are detected.
Ramping up TBHT to 230A max and TGHT to achieve ~1900C
Wednesday, October 07, 2015, 11:12
Yesterday...
TBHT ramped up to 230A and TGHT was at 160A before taking temperature readings.
TGHT from 160A to 423A, IR2C temp reading increases linearly from 1138C to 1900C, whereas the thermocouple readouts are not quite linear, 1040C to 1748C (see attachment)
After 18 hours, both temp reader dropped about 45C.
Increased TGHT to 440C, IR2C & thermocouple currently read 1912C & 1762C, respectively.
Wednesday, October 07, 2015, 12:28
Lowered TBHT to 200A and TGHT remained at 440A. IR2C = 1900C, TypeC = 1745C. Not much affect from TBHT.
Will increase TBHT back to 230A, then start ramping down TGHT and taking temp readings.
Wednesday, October 07, 2015, 17:49
Stepped down TGHT to 160A and TBHT stayed at 230A. Cooling down temp is generated. See attachment.
Notice the overall temp during cooling is lower than that during heating.
TGHT and TBHT will be ramped down to 0A.
Chamber will be vented tomorrow.
More details later...
|
Thursday, October 08, 2015, 12:26, John Wong, Empty, 41077-5, LP-SIS, In progress, Test#2: Measuring temp with thermocouple (away from centre) & 2C-IR
|
John Wong wrote: |
John Wong wrote: |
Laura Lambert wrote: |
Thursday, September 24, 2015, 08:39
IGP1 = 6.5e-7Torr
HS water valves opened, no leaks detected.
Tapped up manually to 35A.
Waited ~20min.
Vacuum stable, IGP1 = 1.5e-6 Torr.
Initiated auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively with final setpoints of 250A and 230A.
Final temp of 1200C on auto-ramp in order to initiate temperature measurements starting at ~1200C.
Thursday, September 24, 2015, 10:24
IGP1 = 8.7e-7 Torr
TGHT = 44A, TBHT = 38A
Increasing auto-ramp to 0.5A/min and 0.2A/min for the TGHT and TBHT respectively.
|
Thursday, September 24, 2015, 12:04
A few notes about the target container:The Ta-foil is cut in a full length of the target container, and that also covers up the back block, and the container is wrapped with 3 sheets (see attachment)
The inner tube is coated with TaC, using the "flushing technique" - the coating looks much better; will see how it turns out after the sintering process
The target will be heated up to 1900C . Due to the new wrapping of the Ta-heat shield, the heat distribution may be different. So the target heater will be ramped up to achieve the desired temperature.
Thursday, September 24, 2015, 18:45
TGHT reached to 250A3.6V, TGHT at 230A and stayed for 1.5 hours. Temp-L = 1280C, Temp-R = 1360C.
Auto-ramp TGHT to 500A at 1A/min and heat at that current for overnight. Will take temp reading tomorrow.
Thursday, September 24, 2015, 23:08
TGHT has reached to 500A/8.57V. Temp-L = 1895C, Temp-R = 2073C. (Not sure why the temperature is real, will need to investigate more to get an absolute temp)
Just to be safe… Ramping down TGHT to 425A (according to e-log id 216, Temp-R reached to 1800C with TGHT at 425A/6.84V, but no temp measured for the left at that time)
Will check again later.
Friday, September 25, 2015, 11:52
The target has been heated at 420A for ~12hours; temp measured ~1900C, slightly higher than the previous target container (W.O#40860-1); the Ta-wraping could affect the heat distribution.
The temperature is also confirmed by using the 2-C digital pyrometer. The tube inner surface is measured about 1900C, and the ionizer tube is about 2400C. (see attachment #2).
Initiating auto-cooling at 2A/min for TGHT and 1A/min for TBHT.
The target will be inspected next Monday
Wednesday, September 30, 2015, 16:01
The target container is fully sintered (see attachment#3)
It is still in the discussion where this container will be used online for the UCx. Nevertheless, the target contain is ready and it looks pretty good.
|
Tuesday, October 06, 2015, 15:09
After further discussion, we are going to reheat this container to 420A. The temperature will be measured with the thermocouple - probe inside the centre of the tube - and the 2C-IR for comparison.
This test is to ensure that the container is actually heated to 1900C before the UCx material can be loaded
The chamber has been pumped down to 1.92e-6 Torr. Heat shield valve is open and no leaks are detected.
Ramping up TBHT to 230A max and TGHT to achieve ~1900C
Wednesday, October 07, 2015, 11:12
Yesterday...
TBHT ramped up to 230A and TGHT was at 160A before taking temperature readings.
TGHT from 160A to 423A, IR2C temp reading increases linearly from 1138C to 1900C, whereas the thermocouple readouts are not quite linear, 1040C to 1748C (see attachment)
After 18 hours, both temp reader dropped about 45C.
Increased TGHT to 440C, IR2C & thermocouple currently read 1912C & 1762C, respectively.
Wednesday, October 07, 2015, 12:28
Lowered TBHT to 200A and TGHT remained at 440A. IR2C = 1900C, TypeC = 1745C. Not much affect from TBHT.
Will increase TBHT back to 230A, then start ramping down TGHT and taking temp readings.
Wednesday, October 07, 2015, 17:49
Stepped down TGHT to 160A and TBHT stayed at 230A. Cooling down temp is generated. See attachment.
Notice the overall temp during cooling is lower than that during heating.
TGHT and TBHT will be ramped down to 0A.
Chamber will be vented tomorrow.
More details later...
|
Thursday, October 08, 2015, 12:01
Test 2: To heat the target container back to ~440A and measure the temperature with the type C thermocouple (inside the tube, away from the centre block) and compared the temp reading with the 2C-IR.
Chamber is currently being pump down, vac at 9e-6 Torr.
Will ramp up TGHT to 160A and TBHT to 230A at 2A/min.
Thursday, October 08, 2015, 17:01
TGHT is now at 440A, TBHT is constant at 230A - IR2C is reading the same as before, 1910C, but Type C is reading lower at 1770C. (see attachment)
Will keep the current at 440A overnight.
Friday, October 09, 2015, 10:06
TGHT has stayed at 440A, TBHT at 230A for ~18hours. R-temp dropped slightly from 1910C to 1890C and typeC dropped from 1770 to 1756; otherwise the measurements are reproducible.
After the group discussion, the online heating curve will be re-calculated based on the temp reading from the IR2C curve.
Next, the target container will be filled with UCx material and the conditioning current for Evap#1 will only go up to 440A (or at least the required current to reach the end of the re-carbonization step).
So pay attention to the current when heating the target up in EVAP#1.
Initiate cooling at 2A/min for TGHT and 1A/min TBHT
Friday, October 09, 2015, 11:35
A note about the voltage that may explain the change in the temperature:
See attachment #2:
Left plot = Test #1:
Initially TGHT ramped up to 423A and temp measured at 1900C. Notice, about an hour later, there was a sudden drop in the voltage, and from thereon, the temp was measured at 1860C. About 18 hours later, TGHT was increased to 440A to achieve 1910C.
Right plot = Test #2
Ramped up TGHT to 440A, temp measured 1910C. At that constant current over the 6 hours period, the voltage slowly increased, and the temperature slightly dropped to 1895C.
|
Tuesday, December 01, 2015, 11:35, Anders Mjos, Empty, 41077-5, LP-SIS, In progress, Test#2: Measuring temp with thermocouple (away from centre) & 2C-IR
|
Data from thermocouple attached. Raw data and Excel sheet with plot. |
Monday, November 30, 2015, 15:38, Laura Lambert, Empty, 39530-9, HP-FEBIAD, Done, emissivity measurements with no h.s on HP-FEBIAD container
|
Monday, November 30, 2015, 15:37
No heat shields.
Container empty.
Loaded into evap2 and currently pumping down.
Tuesday, December 01, 2015, 10:07
HS water valves opened this morning, no leaks detected.
IGP1 = 4.3e-7 Torr.
Slope of OMEGA = 0.98
Tapped up manually to 35A.
Vacuum stable, initiating auto-ramp at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Final setpoints: TBHT = 90A, TGHT = 360A
Once final setpoints reached, will tap up manually to max 1800C [legs = 2000C]
Monday, December 07, 2015, 09:06
Container was tapped up manually with emissivity measurements taken every 50A starting at 360A.
The final measurement was taken at 640A.
Container was ramped down for the weekend.
See attachment for raw data.
|
Monday, November 23, 2015, 14:36, Laura Lambert, Empty, 39530-9, HP-FEBIAD, Done, temp measurements with no h.s on HP-FEBIAD container
|
Monday, November 23, 2015, 14:29
No heat shields.
Container empty.
Loaded into evap2 and currently pumping down.
Tuesday, November 24, 2015, 09:36
HS water valves opened this morning, no leaks detected.
IGP1 = 4.5e-7 Torr.
Changed slope of OMEGA IR to 0.98 for empty container.
Tapped up manually to 35A.
IGP1 = 4.7e-7 Torr.
Vacuum stable, initiating auto-ramp at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Final setpoints: TBHT = 230A, TGHT = 300A
Will tap up manually to 2000C
Tuesday, November 24, 2015, 14:00
TGHT = 300A, 3.75V
TBHT = 230A, 3.08V
IGP1 = 4.7e-7 Torr
No reading yet on the OMEGA.
Re-initiating auto-ramp to final setpoint TGHT = 450A
Wednesday, November 25, 2015, 09:11
IGP1 = 3.0e-7Torr.
TGHT = 450A, 6.37V
Tapping up manually to 2000C
Wednesday, November 25, 2015, 15:31
container was tapped up manually to 650A, slope/emissivity settings were checked.
ramped back down to 450A and tapped up manually while recording data up to 1800C [legs = 2000C]
once reached 1800C, tapped TBHT down manually to see relation of TBHT to temperature/ TGHT
remained at 1800C for ~1hr [while tapping down TBHT] before initiating auto-cool at 2.0A/min for the TGHT
see attachment for raw data.
Thursday, November 26, 2015, 10:08
Vented in air and took out this morning.
|
Tuesday, November 10, 2015, 14:34, Laura Lambert, SiC, 41077-3, LP-SIS, Done, temp measurements with 3xTa h.s on LPSIS (small block) container with SiC
|
Tuesday, November 10, 2015, 14:20
Container previously sintered with TaC coating and temperature measurements taken [see elog ID# 256, 257, 258]
3x Ta heat shields
2 packs of 5 SiC discs ~2inches from the end of the right side wrt ionizer tube into page.
Loaded into evap2 and currently pumping down.
see photos attached.
Monday, November 16, 2015, 11:24
HS water valves opened up this morning, no leaks detected.
Tapped up manually to 35A.
Vacuum stable.
IGP1 = 3.4e-7 Torr.
Initiating auto-ramp at 1.0A/min and 0.5A/min for the TGHT and TBHT respectively.
Final setpoints: 250A for the TGHT and 230A for the TBHT
Monday, November 16, 2015, 13:29
Vacuum too high.
IGP1 = 2.9e-5 Torr.
Decreasing ramping rate down to 0.5A/min and 0.2A/min for the TGHT and TBHT respectively.
Tuesday, November 17, 2015, 09:12
IGP1 = 1.45e-7 Torr.
TGHT = 250A, 3.28V
TBHT = 230A, 3.33V
OMEGA = 1194C
Tapping up manually to 1900C
Tuesday, November 17, 2015, 11:22
Tapped up manually to 1800C, realized SiC should only be tapped up to 1700C, backed off immediately down to 415A from 460A/ 1800C.
See attachment for photo of striptool/ time spent above 1700C [~20min].
Tuesday, November 17, 2015, 15:46
TGHT remained at 1700C for ~4hrs.
TGHT = 420A, 6.44V.
IGP1 = 2.3e-7 Torr.
Initiating cool-down at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
See attachment for raw data of temperature measurements.
Wednesday, November 18, 2015, 13:32
Vented in air and took out this morning.
Looks good, no visual changes with the container.
|
Thursday, November 05, 2015, 16:20, Laura Lambert, , 41077-3, LP-SIS, In progress, Sintering TaC coating on 'temporary endcaps' springs
|
Thursday, November 05, 2015, 16:19
Springs coated with TaC and loaded into container for sintering.
3x Ta heat shield.
EVAP2 currently pumping down.
Friday, November 06, 2015, 08:39
Opened HS water valves, no leaks detected.
Tapped up manually to 35A.
IGP1 = 5.5e-7 Torr.
Friday, November 06, 2015, 10:08
IGP1 = 5.8e-7 Torr.
Vacuum stable.
Initiating auto-ramp at 0.2A/min and 0.1A/min with final setpoints of 450A and 230A for the TGHT and TBHT respectively.
See photos attached to view how springs were coated and loaded into container.
Monday, November 09, 2015, 09:07
TGHT reached 450A, 7.2V ~8pm sat, nov 7th.
OMEGA = 1775C
IGP1 = 3.2e-7 Torr.
Tapping up manually to 1900C.
|
Monday, November 09, 2015, 12:56, John Wong, , 41077-3, LP-SIS, In progress, Sintering TaC coating on 'temporary endcaps' springs (Slope changed to 1.04)
|
Laura Lambert wrote: |
Thursday, November 05, 2015, 16:19
Springs coated with TaC and loaded into container for sintering.
3x Ta heat shield.
EVAP2 currently pumping down.
Friday, November 06, 2015, 08:39
Opened HS water valves, no leaks detected.
Tapped up manually to 35A.
IGP1 = 5.5e-7 Torr.
Friday, November 06, 2015, 10:08
IGP1 = 5.8e-7 Torr.
Vacuum stable.
Initiating auto-ramp at 0.2A/min and 0.1A/min with final setpoints of 450A and 230A for the TGHT and TBHT respectively.
See photos attached to view how springs were coated and loaded into container.
Monday, November 09, 2015, 09:07
TGHT reached 450A, 7.2V ~8pm sat, nov 7th.
OMEGA = 1775C
IGP1 = 3.2e-7 Torr.
Tapping up manually to 1900C.
|
Monday, November 09, 2015, 12:30
Checked the temp on the inner surface (not at the spring) of the container was around 2050C at 500A.
The TaC coated spring is reading at 1900C; that's what the OMEGA is reading with the setting for 2-colors and slope at 0.98.
Lower TGHT to 450A/ 7.12V.
By comparing the data from the previous temp curve (OMEGA slope at 0.98) with no material inside the container, the voltage and current plot is aligned with the curve.
Changed OMEGA setting slope to 1.04. Current temp is reading at 1917C at 450A.
For 2-Color setting, the emissivity should be negligible. That makes me believe that different materials has different slope setting for the temp reading.
One thing to note is that, the sintering temp of TaC is around 1900-2000C. It was clear that the container was fully sintered with TGHT at 450A.
Will need to gather more data with different material to understand the slope setting better.
Try:
SiC at 1700C, slope at 1.04
ZrC at 1900C, slope at 104
Ta at 1900C, slope at 0.98.
Compare the data...
|
Monday, November 09, 2015, 14:22, Laura Lambert, , 41077-3, LP-SIS, Done, Sintering TaC coating on 'temporary endcaps' springs (Slope changed to 1.04)
|
John Wong wrote: |
Laura Lambert wrote: |
Thursday, November 05, 2015, 16:19
Springs coated with TaC and loaded into container for sintering.
3x Ta heat shield.
EVAP2 currently pumping down.
Friday, November 06, 2015, 08:39
Opened HS water valves, no leaks detected.
Tapped up manually to 35A.
IGP1 = 5.5e-7 Torr.
Friday, November 06, 2015, 10:08
IGP1 = 5.8e-7 Torr.
Vacuum stable.
Initiating auto-ramp at 0.2A/min and 0.1A/min with final setpoints of 450A and 230A for the TGHT and TBHT respectively.
See photos attached to view how springs were coated and loaded into container.
Monday, November 09, 2015, 09:07
TGHT reached 450A, 7.2V ~8pm sat, nov 7th.
OMEGA = 1775C
IGP1 = 3.2e-7 Torr.
Tapping up manually to 1900C.
|
Monday, November 09, 2015, 12:30
Checked the temp on the inner surface (not at the spring) of the container was around 2050C at 500A.
The TaC coated spring is reading at 1900C; that's what the OMEGA is reading with the setting for 2-colors and slope at 0.98.
Lower TGHT to 450A/ 7.12V.
By comparing the data from the previous temp curve (OMEGA slope at 0.98) with no material inside the container, the voltage and current plot is aligned with the curve.
Changed OMEGA setting slope to 1.04. Current temp is reading at 1917C at 450A.
For 2-Color setting, the emissivity should be negligible. That makes me believe that different materials has different slope setting for the temp reading.
One thing to note is that, the sintering temp of TaC is around 1900-2000C. It was clear that the container was fully sintered with TGHT at 450A.
Will need to gather more data with different material to understand the slope setting better.
Try:
SiC at 1700C, slope at 1.04
ZrC at 1900C, slope at 104
Ta at 1900C, slope at 0.98.
Compare the data...
|
Monday, November 09, 2015, 14:20
IGP1 = 3.3e-7 Torr.
TGHT = 450A, 7.12V
OMEGA = 1915C
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Tuesday, November 10, 2015, 13:23
Vented and opened this morning.
springs look [mostly] sintered.
see photo attached.
|
Monday, November 02, 2015, 16:29, Laura Lambert, Empty, 41077-3, LP-SIS, Done, temp measurements with 3xTa h.s on LPSIS (small block) container
|
Monday, November 02, 2015, 16:28
Container previously sintered with TaC coating and temperature measurements taken with 1x Ta heat shield [see elog ID# 256] and 2x Ta heat shield [see elog ID#257]
3x Ta heat shields on this container.
Loaded into evap2 and currently pumping down.
Tuesday, November 03, 2015, 10:37
HS water valves opened up this morning, no leaks detected.
Tapped up manually to 35A.
Vacuum stable.
IGP1 = 6.8e-7 Torr.
Initiating auto-ramp at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Final setpoints: 250A for the TGHT and 230A for the TBHT
Tuesday, November 03, 2015, 13:09
IGP1 = 7.7e-7 Torr
TGHT = 250A, 3.42V
TBHT = 185A, 3.0V
OMEGA = 1237C
Increasing ramping rate of TBHT to 2.0A/min.
Tuesday, November 03, 2015, 13:47
Reached final setpoints.
IGP1 = 8.7e-7 Torr.
Tapping up manually to 1900C
Tuesday, November 03, 2015, 15:45
Tapped up manually to 1900C
TGHT = 450A, 7.26V
IGP1 = 1.6e-6 Torr
Will remain at 450A overnight and ramp-down in the morning.
Wednesday, November 04, 2015, 10:00
TGHT remained at 450A for ~18hrs.
IGP1 = 6e-7 Torr.
OMEGA = 1908C
See attachment for raw data of temperature measurements and picture showing voltage movement at max setpoint.
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Wednesday, November 04, 2015, 16:43
Vented and took out this afternoon.
Container looks good.
No visible changes to container compared to 2xTa heat shield temp measurements.
|
Monday, October 26, 2015, 16:17, Laura Lambert, Empty, 41077-3, LP-SIS, Done, temp measurements with 2xTa h.s on LPSIS (small block) container 6x
|
Monday, October 26, 2015, 16:16
Container previously sintered with TaC coating and temperature measurements taken with 1x Ta heat shield [see elog ID# 256]
2x Ta heat shields on this container.
Loaded into evap2 and currently pumping down.
Tuesday, October 27, 2015, 10:07
HS water valves opened up this morning, no leaks detected.
Tapped up manually to 35A.
Waited ~10min, vacuum stable
Initiating auto-ramp at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Final setpoints: 300A for the TGHT and 230A for the TBHT
Tuesday, October 27, 2015, 13:54
Reached final setpoints.
IGP1 = 5.3e-7 Torr.
Tapping up manually to 1900C
Tuesday, October 27, 2015, 16:42
Tapped up manually to 1900C
TGHT = 455A, 7.66V
IGP1 = 9e-7 Torr
Will remain at 455A overnight and ramp-down in the morning.
Wednesday, October 28, 2015, 09:32
TGHT remained at 455A for ~17hrs.
IGP1 = 4.3e-7 Torr.
OMEGA = 1888C
See attachment for raw data of temperature measurements.
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Wednesday, October 28, 2015, 16:32
Vented and took out this afternoon.
Container looks good.
See photos attached.
|
Wednesday, October 21, 2015, 17:39, John Wong, Empty, 41077-3, LP-SIS, In progress, Sintering TaC on LPSIS (small block) container
|
Wednesday, October 21, 2015, 17:35
This container is prepared for a backup UCx target (otherwise it will be used for development purposes).
The container is coated with TaC; one layer of Ta-heat shield is used.
TGHT will be ramped up to reach 1900C (previous container had TGHT ramped up to 440A).
TBHT will be ramped up to max 230A.
Chamber is currently being pumped down.
Heating can begin once the vacuum is good, currently at 4.8e-5 Torr.
Friday, October 23, 2015, 16:15
TGHT reached to 500A and temp measured at 1940C. More about the temp plot can be found in the dropbox.
Initiated cooling down at 2A/min.
Target will be inspected next Monday.
|
Thursday, October 22, 2015, 11:41, Laura Lambert, Empty, 41077-3, LP-SIS, In progress, Sintering TaC on LPSIS (small block) container
|
John Wong wrote: |
Wednesday, October 21, 2015, 17:35
This container is prepared for a backup UCx target (otherwise it will be used for development purposes).
The container is coated with TaC; one layer of Ta-heat shield is used.
TGHT will be ramped up to reach 1900C (previous container had TGHT ramped up to 440A).
TBHT will be ramped up to max 230A.
Chamber is currently being pumped down.
Heating can begin once the vacuum is good, currently at 4.8e-5 Torr.
|
Thursday, October 22, 2015, 11:36
HS water valves opened, no leaks detected.
Tapped up manually to 35A.
Vacuum stabilized, initiated auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
Final setpoints TGHT = 300A, TBHT = 230A
IGP1 = 1.0e-6 Torr; TGHT = 45.18A, 0.17V; TBHT = 38.4A, 0.41V
|
Thursday, October 22, 2015, 17:10, John Wong, Empty, 41077-3, LP-SIS, In progress, Sintering TaC on LPSIS (small block) container
|
Laura Lambert wrote: |
John Wong wrote: |
Wednesday, October 21, 2015, 17:35
This container is prepared for a backup UCx target (otherwise it will be used for development purposes).
The container is coated with TaC; one layer of Ta-heat shield is used.
TGHT will be ramped up to reach 1900C (previous container had TGHT ramped up to 440A).
TBHT will be ramped up to max 230A.
Chamber is currently being pumped down.
Heating can begin once the vacuum is good, currently at 4.8e-5 Torr.
|
Thursday, October 22, 2015, 11:36
HS water valves opened, no leaks detected.
Tapped up manually to 35A.
Vacuum stabilized, initiated auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
Final setpoints TGHT = 300A, TBHT = 230A
IGP1 = 1.0e-6 Torr; TGHT = 45.18A, 0.17V; TBHT = 38.4A, 0.41V
|
Thursday, October 22, 2015, 17:09
Pressure coming down to 1.5e-6 Torr.
Increased ramping rate to 2A/min for both TGHT and TBHT.
|
Monday, October 26, 2015, 16:14, Laura Lambert, Empty, 41077-3, LP-SIS, Done, Sintering TaC on LPSIS (small block) container & temp measurements with 1xTa h.s
|
John Wong wrote: |
Laura Lambert wrote: |
John Wong wrote: |
Wednesday, October 21, 2015, 17:35
This container is prepared for a backup UCx target (otherwise it will be used for development purposes).
The container is coated with TaC; one layer of Ta-heat shield is used.
TGHT will be ramped up to reach 1900C (previous container had TGHT ramped up to 440A).
TBHT will be ramped up to max 230A.
Chamber is currently being pumped down.
Heating can begin once the vacuum is good, currently at 4.8e-5 Torr.
|
Thursday, October 22, 2015, 11:36
HS water valves opened, no leaks detected.
Tapped up manually to 35A.
Vacuum stabilized, initiated auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
Final setpoints TGHT = 300A, TBHT = 230A
IGP1 = 1.0e-6 Torr; TGHT = 45.18A, 0.17V; TBHT = 38.4A, 0.41V
|
Thursday, October 22, 2015, 17:09
Pressure coming down to 1.5e-6 Torr.
Increased ramping rate to 2A/min for both TGHT and TBHT.
|
Monday, October 26, 2015, 16:10
Target container was ramped down over the weekend and taken out today.
Coating looks good.
Will add on another Ta layer and continue with temperature measurements.
See attachment for raw data.
|
Tuesday, September 01, 2015, 17:20, John Wong, SiC, 39530-5, HP-FEBIAD, In progress, Sintering SiC#32
|
Tuesday, September 01, 2015, 17:16
Target container contains 533 discs of SiC with packed length of 17cm.
Mass of 533 discs SiC(green) = 57.8979g
Total mass SiC(green) + target container = 1455g
Container is wrapped with 3 heatshields; no end caps are inserted yet.
Sintering temp at 1800C - TGHT will be set accordingly. TBHT max at 230A.
Chamber is currently being pumped down.
|
Wednesday, September 02, 2015, 11:28, Laura Lambert, SiC, 39530-5, HP-FEBIAD, In progress, Sintering SiC#32
|
John Wong wrote: |
Tuesday, September 01, 2015, 17:16
Target container contains 533 discs of SiC with packed length of 17cm.
Mass of 533 discs SiC(green) = 57.8979g
Total mass SiC(green) + target container = 1455g
Container is wrapped with 3 heatshields; no end caps are inserted yet.
Sintering temp at 1800C - TGHT will be set accordingly. TBHT max at 230A.
Chamber is currently being pumped down.
|
Wednesday, September 02, 2015, 09:11
HS water valves opened, no leaks detected.
IGP1 = 1.15e-6 Torr
Tapped up manually to 40A.
Waited ~1hr40 for vacuum to stabilize.
IGP1 = 3.6e-6 Torr.
Max setpoints set to TGHT = 630A and TBHT = 230A, ~1400C
Initiating auto ramp at a rate of 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
Once max setpoints achieved, will tap up manually until window port becomes coated [as previously observed]
Once window port becomes coated will leave at set temp for ~4hrs to continue with outgassing, then cool down, clean window and ramp back up.
If LS port still clean, will continue to ramp up to final desired temperature of 1800C.
Wednesday, September 02, 2015, 14:23
IGP1 = 4.0e-5 Torr.
Vacuum too high, stopped auto-ramp and tapped down manually.
Dropped TGHT down from 80A to 50A
Dropped TBHT down from 55A to 50A
Wednesday, September 02, 2015, 15:29
Vacuum down to IGP1 = 1.2e-5 Torr.
Re-initiating auto-ramp...
Tuesday, September 08, 2015, 10:04
IGP1 = 4.5e-7 Torr.
TGHT = 630A, 9.6V
TBHT = 230A, 3.2V
DV = 0.22V
OMEGA RS = 1476C
OMEGA LS = 1450C
see attached photo for screenshot.
will tap up manually with a visual on both window ports...
|
Tuesday, September 08, 2015, 15:56, John Wong, SiC, 39530-5, HP-FEBIAD, In progress, Sintering SiC#32
|
Laura Lambert wrote: |
John Wong wrote: |
Tuesday, September 01, 2015, 17:16
Target container contains 533 discs of SiC with packed length of 17cm.
Mass of 533 discs SiC(green) = 57.8979g
Total mass SiC(green) + target container = 1455g
Container is wrapped with 3 heatshields; no end caps are inserted yet.
Sintering temp at 1800C - TGHT will be set accordingly. TBHT max at 230A.
Chamber is currently being pumped down.
|
Wednesday, September 02, 2015, 09:11
HS water valves opened, no leaks detected.
IGP1 = 1.15e-6 Torr
Tapped up manually to 40A.
Waited ~1hr40 for vacuum to stabilize.
IGP1 = 3.6e-6 Torr.
Max setpoints set to TGHT = 630A and TBHT = 230A, ~1400C
Initiating auto ramp at a rate of 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
Once max setpoints achieved, will tap up manually until window port becomes coated [as previously observed]
Once window port becomes coated will leave at set temp for ~4hrs to continue with outgassing, then cool down, clean window and ramp back up.
If LS port still clean, will continue to ramp up to final desired temperature of 1800C.
Wednesday, September 02, 2015, 14:23
IGP1 = 4.0e-5 Torr.
Vacuum too high, stopped auto-ramp and tapped down manually.
Dropped TGHT down from 80A to 50A
Dropped TBHT down from 55A to 50A
Wednesday, September 02, 2015, 15:29
Vacuum down to IGP1 = 1.2e-5 Torr.
Re-initiating auto-ramp...
Tuesday, September 08, 2015, 10:04
IGP1 = 4.5e-7 Torr.
TGHT = 630A, 9.6V
TBHT = 230A, 3.2V
DV = 0.22V
OMEGA RS = 1476C
OMEGA LS = 1450C
see attached photo for screenshot.
will tap up manually with a visual on both window ports...
|
Tuesday, September 08, 2015, 15:44
TGHT has stepped up to 820A. Coating on both windows is becoming obvious and it's interfering the temp readers; however, the left window (see attachment, which is further away from the target) is lightly coated than the right. See attachment for The Temp (and Power) vs current plots.
Target will remained heated at the current and will be cooled down later today.
The target will be re-conditioned up to 820A and temp and mass will be re-measured.
Plans:
The chamber will be vented tomorrow and the target will be taken out to weigh for mass change.
The chamber windows will need to be clean.
A piece of Ta foil will be cover in front of the ionizer to trap any loss material (if any).
Tuesday, September 08, 2015, 17:37
TGHT was at 800A for 2 hours before ramping up 820A for another 2 hours heating. More coating on the right window is observed and temp reading came down to 1340C. The left window remains the same and temp reads at 1646C.
Ramping TGHT/TBHT to 0A at 2A/min and 1A/min, respectively.
Wednesday, September 09, 2015, 12:27
Result after the sintering process:
No yellow crystal formed (compared to previously observed SiC targets that heated up above 1900C).
Total green mass = 57.90g
mass of graphite foil = 0.035g x 533 discs = 18.7g
mass of green SiC = 39.30g
Target container with SiC before sintered = 1455g
Target container after sintered = 1450g
mass loss ~ 5.0g ~ 13% organic mass, as expected!
The target will undergo the re-condition stage, and the temperature will be measured from 600A to 820A.
|
Wednesday, September 09, 2015, 18:24, John Wong, SiC, 39530-5, HP-FEBIAD, In progress, Re-conditioning SiC#32
|
John Wong wrote: |
Laura Lambert wrote: |
John Wong wrote: |
Tuesday, September 01, 2015, 17:16
Target container contains 533 discs of SiC with packed length of 17cm.
Mass of 533 discs SiC(green) = 57.8979g
Total mass SiC(green) + target container = 1455g
Container is wrapped with 3 heatshields; no end caps are inserted yet.
Sintering temp at 1800C - TGHT will be set accordingly. TBHT max at 230A.
Chamber is currently being pumped down.
|
Wednesday, September 02, 2015, 09:11
HS water valves opened, no leaks detected.
IGP1 = 1.15e-6 Torr
Tapped up manually to 40A.
Waited ~1hr40 for vacuum to stabilize.
IGP1 = 3.6e-6 Torr.
Max setpoints set to TGHT = 630A and TBHT = 230A, ~1400C
Initiating auto ramp at a rate of 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
Once max setpoints achieved, will tap up manually until window port becomes coated [as previously observed]
Once window port becomes coated will leave at set temp for ~4hrs to continue with outgassing, then cool down, clean window and ramp back up.
If LS port still clean, will continue to ramp up to final desired temperature of 1800C.
Wednesday, September 02, 2015, 14:23
IGP1 = 4.0e-5 Torr.
Vacuum too high, stopped auto-ramp and tapped down manually.
Dropped TGHT down from 80A to 50A
Dropped TBHT down from 55A to 50A
Wednesday, September 02, 2015, 15:29
Vacuum down to IGP1 = 1.2e-5 Torr.
Re-initiating auto-ramp...
Tuesday, September 08, 2015, 10:04
IGP1 = 4.5e-7 Torr.
TGHT = 630A, 9.6V
TBHT = 230A, 3.2V
DV = 0.22V
OMEGA RS = 1476C
OMEGA LS = 1450C
see attached photo for screenshot.
will tap up manually with a visual on both window ports...
|
Tuesday, September 08, 2015, 15:44
TGHT has stepped up to 820A. Coating on both windows is becoming obvious and it's interfering the temp readers; however, the left window (see attachment, which is further away from the target) is lightly coated than the right. See attachment for The Temp (and Power) vs current plots.
Target will remained heated at the current and will be cooled down later today.
The target will be re-conditioned up to 820A and temp and mass will be re-measured.
Plans:
The chamber will be vented tomorrow and the target will be taken out to weigh for mass change.
The chamber windows will need to be clean.
A piece of Ta foil will be cover in front of the ionizer to trap any loss material (if any).
Tuesday, September 08, 2015, 17:37
TGHT was at 800A for 2 hours before ramping up 820A for another 2 hours heating. More coating on the right window is observed and temp reading came down to 1340C. The left window remains the same and temp reads at 1646C.
Ramping TGHT/TBHT to 0A at 2A/min and 1A/min, respectively.
Wednesday, September 09, 2015, 12:27
Result after the sintering process:
No yellow crystal formed (compared to previously observed SiC targets that heated up above 1900C).
Total green mass = 57.90g
mass of graphite foil = 0.035g x 533 discs = 18.7g
mass of green SiC = 39.30g
Target container with SiC before sintered = 1455g
Target container after sintered = 1450g
mass loss ~ 5.0g ~ 13% organic mass, as expected!
The target will undergo the re-condition stage, and the temperature will be measured from 600A to 820A.
|
Wednesday, September 09, 2015, 17:39
Both end-caps are inserted onto the targets. The total mass (Target, Sintered SiC, end caps, 4x 19"round graphite foils) = 1453g.
Target is wrapped with 3 layers of heat shields.
The extraction electrode is wrapped with Ta-foil (see attachment). This is to trap any lose particle, if any.
Chamber is currently being pumped down, currently at 1.2e-5 Torr.
|
Thursday, September 10, 2015, 09:58, Laura Lambert, SiC, 39530-5, HP-FEBIAD, In progress, Re-conditioning SiC#32
|
John Wong wrote: |
John Wong wrote: |
Laura Lambert wrote: |
John Wong wrote: |
Tuesday, September 01, 2015, 17:16
Target container contains 533 discs of SiC with packed length of 17cm.
Mass of 533 discs SiC(green) = 57.8979g
Total mass SiC(green) + target container = 1455g
Container is wrapped with 3 heatshields; no end caps are inserted yet.
Sintering temp at 1800C - TGHT will be set accordingly. TBHT max at 230A.
Chamber is currently being pumped down.
|
Wednesday, September 02, 2015, 09:11
HS water valves opened, no leaks detected.
IGP1 = 1.15e-6 Torr
Tapped up manually to 40A.
Waited ~1hr40 for vacuum to stabilize.
IGP1 = 3.6e-6 Torr.
Max setpoints set to TGHT = 630A and TBHT = 230A, ~1400C
Initiating auto ramp at a rate of 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
Once max setpoints achieved, will tap up manually until window port becomes coated [as previously observed]
Once window port becomes coated will leave at set temp for ~4hrs to continue with outgassing, then cool down, clean window and ramp back up.
If LS port still clean, will continue to ramp up to final desired temperature of 1800C.
Wednesday, September 02, 2015, 14:23
IGP1 = 4.0e-5 Torr.
Vacuum too high, stopped auto-ramp and tapped down manually.
Dropped TGHT down from 80A to 50A
Dropped TBHT down from 55A to 50A
Wednesday, September 02, 2015, 15:29
Vacuum down to IGP1 = 1.2e-5 Torr.
Re-initiating auto-ramp...
Tuesday, September 08, 2015, 10:04
IGP1 = 4.5e-7 Torr.
TGHT = 630A, 9.6V
TBHT = 230A, 3.2V
DV = 0.22V
OMEGA RS = 1476C
OMEGA LS = 1450C
see attached photo for screenshot.
will tap up manually with a visual on both window ports...
|
Tuesday, September 08, 2015, 15:44
TGHT has stepped up to 820A. Coating on both windows is becoming obvious and it's interfering the temp readers; however, the left window (see attachment, which is further away from the target) is lightly coated than the right. See attachment for The Temp (and Power) vs current plots.
Target will remained heated at the current and will be cooled down later today.
The target will be re-conditioned up to 820A and temp and mass will be re-measured.
Plans:
The chamber will be vented tomorrow and the target will be taken out to weigh for mass change.
The chamber windows will need to be clean.
A piece of Ta foil will be cover in front of the ionizer to trap any loss material (if any).
Tuesday, September 08, 2015, 17:37
TGHT was at 800A for 2 hours before ramping up 820A for another 2 hours heating. More coating on the right window is observed and temp reading came down to 1340C. The left window remains the same and temp reads at 1646C.
Ramping TGHT/TBHT to 0A at 2A/min and 1A/min, respectively.
Wednesday, September 09, 2015, 12:27
Result after the sintering process:
No yellow crystal formed (compared to previously observed SiC targets that heated up above 1900C).
Total green mass = 57.90g
mass of graphite foil = 0.035g x 533 discs = 18.7g
mass of green SiC = 39.30g
Target container with SiC before sintered = 1455g
Target container after sintered = 1450g
mass loss ~ 5.0g ~ 13% organic mass, as expected!
The target will undergo the re-condition stage, and the temperature will be measured from 600A to 820A.
|
Wednesday, September 09, 2015, 17:39
Both end-caps are inserted onto the targets. The total mass (Target, Sintered SiC, end caps, 4x 19"round graphite foils) = 1453g.
Target is wrapped with 3 layers of heat shields.
The extraction electrode is wrapped with Ta-foil (see attachment). This is to trap any lose particle, if any.
Chamber is currently being pumped down, currently at 1.2e-5 Torr.
|
Thursday, September 10, 2015, 09:55
HS water valves opened this morning, no leaks detected.
TGHT and TBHT tapped up manually to 35A.
IGP1 = 4.4e-7 Torr, vacuum stable.
Initiating auto-ramp at 1.0A/min and 0.5A/min for the TGHT and TBHT respectively with final setpoints of 600A and 230A.
|
Thursday, September 10, 2015, 12:05, John Wong, SiC, 39530-5, HP-FEBIAD, Done, Re-conditioning SiC#32
|
Laura Lambert wrote: |
John Wong wrote: |
John Wong wrote: |
Laura Lambert wrote: |
John Wong wrote: |
Tuesday, September 01, 2015, 17:16
Target container contains 533 discs of SiC with packed length of 17cm.
Mass of 533 discs SiC(green) = 57.8979g
Total mass SiC(green) + target container = 1455g
Container is wrapped with 3 heatshields; no end caps are inserted yet.
Sintering temp at 1800C - TGHT will be set accordingly. TBHT max at 230A.
Chamber is currently being pumped down.
|
Wednesday, September 02, 2015, 09:11
HS water valves opened, no leaks detected.
IGP1 = 1.15e-6 Torr
Tapped up manually to 40A.
Waited ~1hr40 for vacuum to stabilize.
IGP1 = 3.6e-6 Torr.
Max setpoints set to TGHT = 630A and TBHT = 230A, ~1400C
Initiating auto ramp at a rate of 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
Once max setpoints achieved, will tap up manually until window port becomes coated [as previously observed]
Once window port becomes coated will leave at set temp for ~4hrs to continue with outgassing, then cool down, clean window and ramp back up.
If LS port still clean, will continue to ramp up to final desired temperature of 1800C.
Wednesday, September 02, 2015, 14:23
IGP1 = 4.0e-5 Torr.
Vacuum too high, stopped auto-ramp and tapped down manually.
Dropped TGHT down from 80A to 50A
Dropped TBHT down from 55A to 50A
Wednesday, September 02, 2015, 15:29
Vacuum down to IGP1 = 1.2e-5 Torr.
Re-initiating auto-ramp...
Tuesday, September 08, 2015, 10:04
IGP1 = 4.5e-7 Torr.
TGHT = 630A, 9.6V
TBHT = 230A, 3.2V
DV = 0.22V
OMEGA RS = 1476C
OMEGA LS = 1450C
see attached photo for screenshot.
will tap up manually with a visual on both window ports...
|
Tuesday, September 08, 2015, 15:44
TGHT has stepped up to 820A. Coating on both windows is becoming obvious and it's interfering the temp readers; however, the left window (see attachment, which is further away from the target) is lightly coated than the right. See attachment for The Temp (and Power) vs current plots.
Target will remained heated at the current and will be cooled down later today.
The target will be re-conditioned up to 820A and temp and mass will be re-measured.
Plans:
The chamber will be vented tomorrow and the target will be taken out to weigh for mass change.
The chamber windows will need to be clean.
A piece of Ta foil will be cover in front of the ionizer to trap any loss material (if any).
Tuesday, September 08, 2015, 17:37
TGHT was at 800A for 2 hours before ramping up 820A for another 2 hours heating. More coating on the right window is observed and temp reading came down to 1340C. The left window remains the same and temp reads at 1646C.
Ramping TGHT/TBHT to 0A at 2A/min and 1A/min, respectively.
Wednesday, September 09, 2015, 12:27
Result after the sintering process:
No yellow crystal formed (compared to previously observed SiC targets that heated up above 1900C).
Total green mass = 57.90g
mass of graphite foil = 0.035g x 533 discs = 18.7g
mass of green SiC = 39.30g
Target container with SiC before sintered = 1455g
Target container after sintered = 1450g
mass loss ~ 5.0g ~ 13% organic mass, as expected!
The target will undergo the re-condition stage, and the temperature will be measured from 600A to 820A.
|
Wednesday, September 09, 2015, 17:39
Both end-caps are inserted onto the targets. The total mass (Target, Sintered SiC, end caps, 4x 19"round graphite foils) = 1453g.
Target is wrapped with 3 layers of heat shields.
The extraction electrode is wrapped with Ta-foil (see attachment). This is to trap any lose particle, if any.
Chamber is currently being pumped down, currently at 1.2e-5 Torr.
|
Thursday, September 10, 2015, 09:55
HS water valves opened this morning, no leaks detected.
TGHT and TBHT tapped up manually to 35A.
IGP1 = 4.4e-7 Torr, vacuum stable.
Initiating auto-ramp at 1.0A/min and 0.5A/min for the TGHT and TBHT respectively with final setpoints of 600A and 230A.
|
Thursday, September 10, 2015, 12:05
Changed TGHT to 2A/min and TGHT remains at 1A/min. Vacuum is table at 1.0e-6 Torr.
Friday, September 11, 2015, 11:34
TGHT was at 600A for almost 20 hours. Vac at 5.2 e-7 Torr. L-temp at 1490C, R-temp at 1685 (odd?). Using pyrometer to measure - Right end does seem brighter than the L end.
Continue to ramp up TGHT. Date is collected, will be posted later.
Friday, September 11, 2015, 11:53
L/R-temp measurements just don't seem normal.
Ramped up to 220A- temp reads L = 1522C, R = 1722C.
Ramping down TBHT doesn't change the temp.
Will cool TGHT/TBHT to 0A at 2A/min & 1A/min, respectively.
Will vent the chamber on Monday and inspect for any wrong.
Monday, September 14, 2015, 12:13
The target has taken out for inspection. No visible damage/problem was observed. The Ta-foil for loss particle capture only showed some heat marking but no material was trapped.
Target was weighted, no mass loss was observed.
Try expending the end caps to get a good thermal conductivity and will re-conditiong again.
Tuesday, September 15, 2015, 12:31
The end caps have been expended.
New Ta foils are used for the heat shields. The foils are cut in 3 1/4" x 12" and wrapped around the target. (see attachment). This is to see if the heat is evenly distributed.
Both omega optical lens are aligned properly.
Target is installed but the chamber is NOT yet being pumped down. Awaiting for the fume hood work in B2 level to be complete before the evaporator can be started.
Wednesday, September 16, 2015, 17:57
The work in the B2 level is done; the nuclear ventilation for the evaporators is now operational.
Chamber is currently being pumped down.
Thursday, September 17, 2015, 12:19
Chamber has been pump down overnight and pressure is currently at 5.8e-7 Torr.
HS valves are opened and no leaks are detected.
Ramping up TGHT/TBHT to 600A at 2A/min and 230A at 1A/min, respectively.
Thursday, September 17, 2015, 17:58
TGHT has reached to 600A/9.14V. Both the L and R temperatures are measured at 1710C and 1760C, respectively. At 600A, the temperature now is about 300C higher compared to that during the sintering process.
The difference in the temperature could be from Ta surface vs SiC surface. (But the 2-color IR temp reader shouldn't matter what color it's measuring?!! I don't know!)
Note:
Both temperature readings are fairly close. Could this be improved from the new Ta-foils? Possible!
It is still unclear what is the absolute temperature. A more systematic student needs to be done.
Using a thermocouple couple to measurement the endcaps at 600A and compared with the Omage reader may help to understand more.
After discussing with Friedhelm, it is decided to stay the target at 600A for the conditioning process.
Friday, September 18, 2015, 09:10
Target has been heated at 600A at stable temperature at 1716C (LS) and 1769C (RS), see attachment.
Friday, September 18, 2015, 11:45
Initiated cooling down at 2A/min for TGHT, and 1A/min TBHT.
Currently vac at 5.48e-7 Torr.
Thursday, September 24, 2015, 11:31
Target was inspected after the 2nd conditioning, up to 1700C at 600A for overnight.
No solid particle was observed that might have extracted from the ionizer tube.
The heat shields have been removed and the target is ready for assembly.
|
Tuesday, August 25, 2015, 11:54, Laura Lambert, Empty, , HP-FEBIAD, In progress, Sintering TaC coating container for SiC Target
|
Tuesday, August 25, 2015, 11:50
Container coated with TaC using new method: Ends tapped off, with liquid poured in and swirled around entire container, then poured back out - 'flushing technique'
Container is wrapped with 3 x Ta heat shields, not incl center block.
Loaded into EVAP2 and currently pumping down.
Tuesday, August 25, 2015, 13:52
IGP1 = 2.2e-6 Torr.
HS water valves opened.
No leaks detected.
Tapped up manually to 35A.
Vacuum stable.
Initiated auto ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
Final setpoints for TGHT = 720A and TBHT = 230A, with final desired temp of 1800C
Wednesday, August 26, 2015, 09:56
IGP1 = 8.8e-7 Torr.
TGHT = 260A, 3.0V
TBHT = 145A, 1.8V
Increasing ramping rate to 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Wednesday, August 26, 2015, 14:15
IGP1 = 3.5e-6 Torr.
TGHT = 720A, 11.3V
TBHT = 230A, 3.2V
DV = 5.48V
OMEGA RS [right side-old port] = 1745C
OMEGA LS [left side-new port] = 1880C
Tapping up manually to achieve 1800C on OMEGA RS
Wednesday, August 26, 2015, 14:44
IGP1 = 3.7e-6 Torr.
TGHT = 748A, 11.9V
DV = 5.78V
OMEGA RS = 1803C
OMEGA LS = 1935C
Thursday, August 27, 2015, 07:31
Remained at max setpoints for ~17hrs.
IGP1 = 1.3e-6 Torr.
DV = 5.79V
OMEGA RS = 1862 [this reading may not be correct due to the laser being moved at max setpoint - this temperature reading may be taken from a different location then the last reading]
OMEGA LS = 1955
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
|
Thursday, August 27, 2015, 16:37, John Wong, Empty, , HP-FEBIAD, Done, Sintering TaC coating container for SiC Target
|
Laura Lambert wrote: |
Tuesday, August 25, 2015, 11:50
Container coated with TaC using new method: Ends tapped off, with liquid poured in and swirled around entire container, then poured back out - 'flushing technique'
Container is wrapped with 3 x Ta heat shields, not incl center block.
Loaded into EVAP2 and currently pumping down.
Tuesday, August 25, 2015, 13:52
IGP1 = 2.2e-6 Torr.
HS water valves opened.
No leaks detected.
Tapped up manually to 35A.
Vacuum stable.
Initiated auto ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
Final setpoints for TGHT = 720A and TBHT = 230A, with final desired temp of 1800C
Wednesday, August 26, 2015, 09:56
IGP1 = 8.8e-7 Torr.
TGHT = 260A, 3.0V
TBHT = 145A, 1.8V
Increasing ramping rate to 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Wednesday, August 26, 2015, 14:15
IGP1 = 3.5e-6 Torr.
TGHT = 720A, 11.3V
TBHT = 230A, 3.2V
DV = 5.48V
OMEGA RS [right side-old port] = 1745C
OMEGA LS [left side-new port] = 1880C
Tapping up manually to achieve 1800C on OMEGA RS
Wednesday, August 26, 2015, 14:44
IGP1 = 3.7e-6 Torr.
TGHT = 748A, 11.9V
DV = 5.78V
OMEGA RS = 1803C
OMEGA LS = 1935C
Thursday, August 27, 2015, 07:31
Remained at max setpoints for ~17hrs.
IGP1 = 1.3e-6 Torr.
DV = 5.79V
OMEGA RS = 1862 [this reading may not be correct due to the laser being moved at max setpoint - this temperature reading may be taken from a different location then the last reading]
OMEGA LS = 1955
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
|
Thursday, August 27, 2015, 16:34
Target is removed from the evaporator and inspected.
The "flushing technique" has a much better result. The inner coated surface is sintered well.
|
Monday, August 24, 2015, 12:58, John Wong, , , , Maintenance, Replacing turbo pump, IEVAP2TP1
|
Monday, August 24, 2015, 12:54
The turbo pump was found to be faulty. The pump couldn't get on full speed and eventually timed out. Vacuum group inspected the pump and it is time for a service.
A new pump has been installed. Leak check was performed and no leaks were detected.
Pump is now fully operational.
Back in business….
|
Tuesday, August 18, 2015, 16:02, Laura Lambert, Ta, , HP-SIS, In progress, Conditioning Ta#46 Target
|
Tuesday, August 18, 2015, 15:53
Target consists of 505 discs.
Total packed length 3.4cm.
Total mass 75.2772g.
Re foil inserted.
3x Ta Heat shields.
No endcaps inserted.
Chamber currently pumping down.
TBHT will be ramped up to 230A at 1.0A/min.
TGHT will be ramped up to 1800C, auto ramp to 600A at 2.0A/min [estimated final value of 720A according to elog ID 184]
*Note: Turbo Pump is on low speed
Wednesday, August 19, 2015, 10:15
IGP1 = 8.3e-7 Torr.
Tapped up manually to 35A.
Initiating auto-ramp.
Wednesday, August 19, 2015, 15:55
IGP1 = 3.3e-6 Torr.
TBHT reached max setpoint of 230A
TGHT reached max setpoint of 600A
OMEGA = 1554C
Increasing final setpoint of TGHT to 700A and re-initiating auto-ramp.
|
Wednesday, August 19, 2015, 17:26, John Wong, Ta, , HP-SIS, In progress, Conditioning Ta#46 Target
|
Laura Lambert wrote: |
Tuesday, August 18, 2015, 15:53
Target consists of 505 discs.
Total packed length 3.4cm.
Total mass 75.2772g.
Re foil inserted.
3x Ta Heat shields.
No endcaps inserted.
Chamber currently pumping down.
TBHT will be ramped up to 230A at 1.0A/min.
TGHT will be ramped up to 1800C, auto ramp to 600A at 2.0A/min [estimated final value of 720A according to elog ID 184]
*Note: Turbo Pump is on low speed
Wednesday, August 19, 2015, 10:15
IGP1 = 8.3e-7 Torr.
Tapped up manually to 35A.
Initiating auto-ramp.
Wednesday, August 19, 2015, 15:55
IGP1 = 3.3e-6 Torr.
TBHT reached max setpoint of 230A
TGHT reached max setpoint of 600A
OMEGA = 1554C
Increasing final setpoint of TGHT to 700A and re-initiating auto-ramp.
|
Wednesday, August 19, 2015, 17:13
TGHT reached to 700A/10.5V, direct voltage at 5.2V, and temp measured at both ends at 1755C. Vac is coming down from 4.2e-6 Torr.
Stepping up TGHT to reach 1800C
Wednesday, August 19, 2015, 17:22
Increased TGHT to 722A/11.3V (direct voltage at 5.48V) to reach 1800C (consistant with the heating curve as for the previous HPTa target, elog 184)
Will continue to condition the target at this temperature for overnight.
Cooling down can be initiated tomorrow morning at 2A/min --- Please measure the target temperature from the new window port before cooling it down.
|
Thursday, August 20, 2015, 10:07, Laura Lambert, Ta, , HP-SIS, In progress, Conditioning Ta#46 Target
|
John Wong wrote: |
Laura Lambert wrote: |
Tuesday, August 18, 2015, 15:53
Target consists of 505 discs.
Total packed length 3.4cm.
Total mass 75.2772g.
Re foil inserted.
3x Ta Heat shields.
No endcaps inserted.
Chamber currently pumping down.
TBHT will be ramped up to 230A at 1.0A/min.
TGHT will be ramped up to 1800C, auto ramp to 600A at 2.0A/min [estimated final value of 720A according to elog ID 184]
*Note: Turbo Pump is on low speed
Wednesday, August 19, 2015, 10:15
IGP1 = 8.3e-7 Torr.
Tapped up manually to 35A.
Initiating auto-ramp.
Wednesday, August 19, 2015, 15:55
IGP1 = 3.3e-6 Torr.
TBHT reached max setpoint of 230A
TGHT reached max setpoint of 600A
OMEGA = 1554C
Increasing final setpoint of TGHT to 700A and re-initiating auto-ramp.
|
Wednesday, August 19, 2015, 17:13
TGHT reached to 700A/10.5V, direct voltage at 5.2V, and temp measured at both ends at 1755C. Vac is coming down from 4.2e-6 Torr.
Stepping up TGHT to reach 1800C
Wednesday, August 19, 2015, 17:22
Increased TGHT to 722A/11.3V (direct voltage at 5.48V) to reach 1800C (consistant with the heating curve as for the previous HPTa target, elog 184)
Will continue to condition the target at this temperature for overnight.
Cooling down can be initiated tomorrow morning at 2A/min --- Please measure the target temperature from the new window port before cooling it down.
|
Thursday, August 20, 2015, 08:27
OMEGA = 1830C
Internal temperature using Mikron taken from the second 'new' view port: Hottest point on target leg = 2250C; hottest point on target material discs inside container = 1830C.
IGP1 = 1.5e-6 Torr.
EVAP2 has been sitting at max setpoints for ~15hours.
Initiated auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
|
Thursday, August 20, 2015, 17:15, John Wong, Ta, , HP-SIS, Done, Conditioning Ta#46 Target
|
Laura Lambert wrote: |
John Wong wrote: |
Laura Lambert wrote: |
Tuesday, August 18, 2015, 15:53
Target consists of 505 discs.
Total packed length 3.4cm.
Total mass 75.2772g.
Re foil inserted.
3x Ta Heat shields.
No endcaps inserted.
Chamber currently pumping down.
TBHT will be ramped up to 230A at 1.0A/min.
TGHT will be ramped up to 1800C, auto ramp to 600A at 2.0A/min [estimated final value of 720A according to elog ID 184]
*Note: Turbo Pump is on low speed
Wednesday, August 19, 2015, 10:15
IGP1 = 8.3e-7 Torr.
Tapped up manually to 35A.
Initiating auto-ramp.
Wednesday, August 19, 2015, 15:55
IGP1 = 3.3e-6 Torr.
TBHT reached max setpoint of 230A
TGHT reached max setpoint of 600A
OMEGA = 1554C
Increasing final setpoint of TGHT to 700A and re-initiating auto-ramp.
|
Wednesday, August 19, 2015, 17:13
TGHT reached to 700A/10.5V, direct voltage at 5.2V, and temp measured at both ends at 1755C. Vac is coming down from 4.2e-6 Torr.
Stepping up TGHT to reach 1800C
Wednesday, August 19, 2015, 17:22
Increased TGHT to 722A/11.3V (direct voltage at 5.48V) to reach 1800C (consistant with the heating curve as for the previous HPTa target, elog 184)
Will continue to condition the target at this temperature for overnight.
Cooling down can be initiated tomorrow morning at 2A/min --- Please measure the target temperature from the new window port before cooling it down.
|
Thursday, August 20, 2015, 08:27
OMEGA = 1830C
Internal temperature using Mikron taken from the second 'new' view port: Hottest point on target leg = 2250C; hottest point on target material discs inside container = 1830C.
IGP1 = 1.5e-6 Torr.
EVAP2 has been sitting at max setpoints for ~15hours.
Initiated auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
|
Thursday, August 20, 2015, 17:14
Target was removed the the evaporator and inspected. It looks good!
Ta-heat shields are removed.
End caps are inserted but need to be expended.
Ready for assembly.
|
Thursday, August 06, 2015, 15:45, Laura Lambert, Endcaps, , TARGET BOAT, Done, Sintering TaC coating on Ta endcaps
|
Thursday, August 06, 2015, 15:36
The endcaps are stacked together with a punched out disc of graphite foil placed in between each endcap for separation so endcaps won't fuse together.
The end caps are further wrapped in a larger piece of graphite foil to hold together as a tube [same method used in elogID # 158]
There are two separate tubes in the target boat:
1) endcaps coated with TaC coating - never been sintered
2) previously sintered [but not fully] endcaps with a second coating done on the one side of each endcap
The boat is wrapped with 3-layers of Ta heatshields.
Chamber is currently being pumped down.
Friday, August 07, 2015, 08:45
HS water valves opened, no leaks detected.
IGP1 = 3.6e-7 Torr.
Tapped up manually to 30A.
Friday, August 07, 2015, 11:23
IGP1 = 2.2e-6 Torr.
Vacuum stable.
Initiating auto-ramp at 0.2A/min with a final setpoint of 480A.
Will ramp up over the weekend, confirm temperature readings on monday and tap up to final desired temperature of 1800C manually.
Friday, August 07, 2015, 13:04
Vacuum climbed quite fast.
IGP1 = 6.3e-6 Torr.
Stopped auto-ramp to allow vacuum to settle.
Waited ~1hr.
IGP1 = 4.3e-6 Torr.
Re-initiating auto-ramp.
Monday, August 10, 2015, 09:22
TGHT reached 480A, 8.2V on the weekend.
OMEGA = 1708C
IGP1 = 3.8e-7 Torr.
Tapped up manually to 1803C, 520A, 9.0V
IGP1 = 5.9e-7 Torr.
Monday, August 10, 2015, 14:50
EVAP2 remained at 1800C for 4.5hours.
Internal temperature taken at new window port read 1800C using the mikron.
Initiating auto-cool at 2.0A/min.
Tuesday, August 11, 2015, 09:23
Vented in air and opened up this morning.
The following observations were noted:
1) single round sintered endcaps:
-Batch of green endcaps, single round of sintering look good. fully sintered.
-however when applying a scratch test, excess TaC scrapes off.
[see single round sintering photos]
2) Re-sintering of batch from july 14th
-Outside of endcap [concave side] was re-coated, Inside of endcap had good first coating - therefore no second coating applied [see photos from elog ID#230]
-A few endcaps almost heated too long and started to appear brittle/ further crystallization on inside of endcap - the side that did not have a second coating applied.
-Outside of endcap looks good/ fully sintered - the side that had a second round of TaC coating
-further tests confirm this batch should still be okay to use
[see round2 batch photos]
|
Friday, July 31, 2015, 15:51, John Wong, Ta, , TARGET BOAT, In progress, Test for homogeneity: Sintering TaC coating on a Ta tube
|
Friday, July 31, 2015, 15:39
A Ta tube was coated with TaC. The inner of the tube was filled with TaC solution and the excess was drained out to give a homogenous coating. The outer layer of the tube was brushed with TaC.
The tube is installed in a target boat and wrapped with 3 layers of heat shields.
Chamber is currently pumped down and the target heater will be ramped up after the long weekend (Tue)
A new window port is installed (see photo). TGHT will need to be ramped up slowly to make sure the new window can sustain the heat shine from the target - local check on the Evap is required to make sure it's safe to keep ramping up the heater.
|
Tuesday, August 04, 2015, 12:04, Laura Lambert, Ta, , TARGET BOAT, Done, Test for homogeneity: Sintering TaC coating on a Ta tube
|
John Wong wrote: |
Friday, July 31, 2015, 15:39
A Ta tube was coated with TaC. The inner of the tube was filled with TaC solution and the excess was drained out to give a homogenous coating. The outer layer of the tube was brushed with TaC.
The tube is installed in a target boat and wrapped with 3 layers of heat shields.
Chamber is currently pumped down and the target heater will be ramped up after the long weekend (Tue)
A new window port is installed (see photo). TGHT will need to be ramped up slowly to make sure the new window can sustain the heat shine from the target - local check on the Evap is required to make sure it's safe to keep ramping up the heater.
|
Tuesday, August 04, 2015, 11:26
HS water valves opened, no leaks detected.
IGP1 = 2.2e-7 Torr.
Tapped up manually to 30A.
IGP1 = 2.7e-7 Torr.
Initiating auto-ramp at 0.2A/min with a final value of 350A.
Tuesday, August 04, 2015, 15:30
IGP1 = 2.8e-6 Torr.
TGHT = 79A.
Increasing ramping rate to 0.5A/min
Wednesday, August 05, 2015, 15:25
EVAP2 reached 350A this morning, OMEGA = 1414C
Temperature measurements were taken using the FLUKE IR camera of the new window port to be used for the second OMEGA camera.
Measurements were taken of both the Cu seal on the inside of the window and in the centre of the window [the hottest point].
TGHT was ramped up at 2.0A/min from 1414C --> 1800C with auto ramp paused at each measurement reading taken.
See attachment for raw data.
TGHT remained at 500A/1800C for 4hrs and will be cooled down at a rate of 2.0A/min.
Thursday, August 06, 2015, 15:32
Vented and opened today.
New window port passed inspection, max temperature reached = 32.4C
Coating on tube looks good, partial sintering. Internal sintered better than outside of tube.
See attached photos.
|
Friday, July 31, 2015, 15:10, John Wong, , , , Maintenance, Installed leftside port
|
Friday, July 31, 2015, 15:09
The left side port was installed on the evaporator #2. Leak check was performed and no leak was detected.
|
Thursday, July 30, 2015, 17:07, John Wong, , , , Maintenance, Connect NALCW to EVAP1
|
Thursday, July 30, 2015, 17:02
EVAP1 cooling system is now on the NALCW. The city water has been removed from the system.
Tested all the cooling system interlocks by shutting off each individual valve, and the main supply valve to the lab - All Passed!
|
Monday, July 13, 2015, 11:54, Laura Lambert, Endcaps, 40282-5, TARGET BOAT, Problems, Sintering TaC coating on Ta endcaps
|
Monday, July 13, 2015, 11:53
A Ta foil is placed in the target boat with separate slots for each endcap [same as elog 200]
The target boat is wrapped with 3-layers of Ta-heat shield.
The boat is installed in EVAP2, chamber is currently being pumped down.
Monday, July 13, 2015, 15:00
Opened HS water valves, no leaks detected.
IGP1 = 2.7e-6 Torr.
Tapping up manually.
Monday, July 13, 2015, 15:41
Tapped up manually to 30A
TGHT = 30A, 0.05V
IGP1 = 7e-6 Torr.
Initiating auto-ramp at 0.2A/min up to 480A with a final desired temperature of 1800C
Tuesday, July 14, 2015, 09:12
IGP1 = 7.8e-7 Torr
TGHT = 241A, 3.3V
OMEGA = 1010C
Increasing auto-ramp to 2.0A/min
Tuesday, July 14, 2015, 11:12
Reached final setpoint of TGHT = 480A, 8.43V
OMEGA = 1667C
IGP1 = 3.3e-6 Torr.
Tapping up manually to reach final desired temperature of 1800C.
Tuesday, July 14, 2015, 11:33
Reached TGHT = 500A, 8.8V by tapping up manually.
OMEGA = 1714V
IGP1= 3.5e-6 Torr.
Re-initiating auto-ramp at 2.0A/min with a final setpoint of 580A.
New final desired temperature min of 1900C
Tuesday, July 14, 2015, 13:16
TGHT = 577A, 10.74V
OMEGA = 1938C
IGP1 = 3.2e-6 Torr
Endcaps have been at this temperature for just over an hour.
Spikes in vacuum started ~430A - this is due to the green TaC coating reacting with the Ta foil, the carbide is reacting directly with the Ta foil [see picture]
Stopping sintering early before endcaps break -> initiating auto-cool at 2.0A/min.
Wednesday, July 15, 2015, 11:33
Vented in air and took out this morning.
Endcaps sintered on top side but not fully sintered on inner edge.
Inner edge is peeling off and unsintered green TaC.
The coating peeling off did not shrink, as seen with previous tests done, one would expect a shrinkage in the coating when heated.
The peeling is most likely due to the way to endcaps were placed in the slots of the Ta foil.
This may have cause the foil to be hotter than the inside of the endcaps and subsequently the Ta foil and TaC coating on the inside reacted - with the Ta foil extracting the carbide from the coating.
This would cause the outer edges of the inside of the endcap to peel/curl inwards as it was heated [like a cast, as the cast dries the outer edges curl inwards].
See photos attached for clarification.
Endcaps will be re-coated and sintered again via a different procedure.
|
Monday, June 29, 2015, 16:18, Laura Lambert, Empty, 41369-2, LP-SIS, In progress, Sintering TaC coating container
|
Monday, June 29, 2015, 16:17
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min.
TBHT will be ramped up to 230A at 01A/min.
Chamber is currently being pumped down.
|
Monday, June 29, 2015, 23:42, John Wong, Empty, 41369-2, LP-SIS, In progress, Sintering TaC coating container
|
Laura Lambert wrote: |
Monday, June 29, 2015, 16:17
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min.
TBHT will be ramped up to 230A at 01A/min.
Chamber is currently being pumped down.
|
Monday, June 29, 2015, 23:37
Opened the HS valves around 5pm. Small leaks or just a vibration in the pipe line caused a rise in vacuum. Leak rate is small, so allow the chamber to continue to pump down over night.
Sintering process can begin tomorrow if vacuum is allowed.
|
Tuesday, June 30, 2015, 09:50, Laura Lambert, Empty, 41369-2, LP-SIS, In progress, Sintering TaC coating container
|
John Wong wrote: |
Laura Lambert wrote: |
Monday, June 29, 2015, 16:17
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min.
TBHT will be ramped up to 230A at 01A/min.
Chamber is currently being pumped down.
|
Monday, June 29, 2015, 23:37
Opened the HS valves around 5pm. Small leaks or just a vibration in the pipe line caused a rise in vacuum. Leak rate is small, so allow the chamber to continue to pump down over night.
Sintering process can begin tomorrow if vacuum is allowed.
|
Tuesday, June 30, 2015, 08:22
IGP1 = 3.6e-7 Torr.
Tapped up manually to 40A.
Vacuum looks good.
IGP1 = 6.9e-7 Torr.
Inititating auto-ramp...
Thursday, July 02, 2015, 09:56
IGP1 = 8.9e-7 Torr.
OMEGA = 1728C
TGHT and TBHT = 580A and 230A respectively.
Tapping up manually to 1800C.
Thursday, July 02, 2015, 11:02
TGHT = 615A, 10.9V
OMEGA = 1800C
IGP1 = 1.1e-6 Torr.
Will continue to heat for 4hrs.
Thursday, July 02, 2015, 15:43
Target container remained at 1800C for 4hrs50min.
Initiating auto-cool for TGHT = 2A/min and TBHT = 1A/min.
Friday, July 03, 2015, 08:24
Vented in air and opened up this morning.
Edge of container on both ends not fully sintered [see photos]
|
Monday, July 06, 2015, 12:07, John Wong, Empty, 41369-2, LP-SIS, In progress, Sintering TaC coating container
|
Laura Lambert wrote: |
John Wong wrote: |
Laura Lambert wrote: |
Monday, June 29, 2015, 16:17
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min.
TBHT will be ramped up to 230A at 01A/min.
Chamber is currently being pumped down.
|
Monday, June 29, 2015, 23:37
Opened the HS valves around 5pm. Small leaks or just a vibration in the pipe line caused a rise in vacuum. Leak rate is small, so allow the chamber to continue to pump down over night.
Sintering process can begin tomorrow if vacuum is allowed.
|
Tuesday, June 30, 2015, 08:22
IGP1 = 3.6e-7 Torr.
Tapped up manually to 40A.
Vacuum looks good.
IGP1 = 6.9e-7 Torr.
Inititating auto-ramp...
Thursday, July 02, 2015, 09:56
IGP1 = 8.9e-7 Torr.
OMEGA = 1728C
TGHT and TBHT = 580A and 230A respectively.
Tapping up manually to 1800C.
Thursday, July 02, 2015, 11:02
TGHT = 615A, 10.9V
OMEGA = 1800C
IGP1 = 1.1e-6 Torr.
Will continue to heat for 4hrs.
Thursday, July 02, 2015, 15:43
Target container remained at 1800C for 4hrs50min.
Initiating auto-cool for TGHT = 2A/min and TBHT = 1A/min.
Friday, July 03, 2015, 08:24
Vented in air and opened up this morning.
Edge of container on both ends not fully sintered [see photos]
|
Monday, July 06, 2015, 11:54
Inner tube surface isn't homogeneously sintered with TaC (see attachment).
A second coating may help.
For the re-sintering process, the target container will be wrapped with 6.2cm Ta (width) foil as a layer for heat shield on each side of the tube, excluding the centre block - just like the same process was done last time, see e-log ID#217.
The Ta-foil and the target tube will be spaced with Ta wire coiled around it.
TGHT can be ramped up about 520A/9.1V to achieve 1900C. Heating time for 3-4 hours until vacuum comes down to low 10-6 Torr.
|
Monday, July 06, 2015, 16:30, Laura Lambert, Empty, 41369-2, LP-SIS, Done, Sintering TaC coating container
|
John Wong wrote: |
Laura Lambert wrote: |
John Wong wrote: |
Laura Lambert wrote: |
Monday, June 29, 2015, 16:17
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min.
TBHT will be ramped up to 230A at 01A/min.
Chamber is currently being pumped down.
|
Monday, June 29, 2015, 23:37
Opened the HS valves around 5pm. Small leaks or just a vibration in the pipe line caused a rise in vacuum. Leak rate is small, so allow the chamber to continue to pump down over night.
Sintering process can begin tomorrow if vacuum is allowed.
|
Tuesday, June 30, 2015, 08:22
IGP1 = 3.6e-7 Torr.
Tapped up manually to 40A.
Vacuum looks good.
IGP1 = 6.9e-7 Torr.
Inititating auto-ramp...
Thursday, July 02, 2015, 09:56
IGP1 = 8.9e-7 Torr.
OMEGA = 1728C
TGHT and TBHT = 580A and 230A respectively.
Tapping up manually to 1800C.
Thursday, July 02, 2015, 11:02
TGHT = 615A, 10.9V
OMEGA = 1800C
IGP1 = 1.1e-6 Torr.
Will continue to heat for 4hrs.
Thursday, July 02, 2015, 15:43
Target container remained at 1800C for 4hrs50min.
Initiating auto-cool for TGHT = 2A/min and TBHT = 1A/min.
Friday, July 03, 2015, 08:24
Vented in air and opened up this morning.
Edge of container on both ends not fully sintered [see photos]
|
Monday, July 06, 2015, 11:54
Inner tube surface isn't homogeneously sintered with TaC (see attachment).
A second coating may help.
For the re-sintering process, the target container will be wrapped with 6.2cm Ta (width) foil as a layer for heat shield on each side of the tube, excluding the centre block - just like the same process was done last time, see e-log ID#217.
The Ta-foil and the target tube will be spaced with Ta wire coiled around it.
TGHT can be ramped up about 520A/9.1V to achieve 1900C. Heating time for 3-4 hours until vacuum comes down to low 10-6 Torr.
|
Monday, July 06, 2015, 16:28
Container has been re-coated with TaC.
Target container is wrapped with a single 15.5cm x 8.5cm Ta foil heat shield on each side of the center block, spaced with Ta wire coil.
Chamber is currently being pumped down.
Tuesday, July 07, 2015, 09:36
HS water valves were opened this morning, no leaks detected.
IGP1 = 6e-7 Torr.
Tapped up manually to 30A.
Waited ~1hr.
Vacuum stable, IGP1 = 1.9e-6 Torr.
Initiating auto-ramp at 0.2A/min and 0.1A/min for TGHT and TBHT respectively.
Target container reached max setpoints of 520A/230A and 1950C ~6hrs ago.
IGP1 = 7.6e-7 Torr.
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
Friday, July 10, 2015, 11:16
Vented in air and removed from evap2.
Again, edges not fully sintered [see photos]
Inside of container looks better, fully coated.
|
Thursday, June 25, 2015, 16:20, Laura Lambert, ZrC, 41177-2, LP-SIS, In progress, Sintering back-up ZrC
|
Thursday, June 25, 2015, 16:14
Total number of foils: 422 discs
Total mass of materials [incl graphite foils]:
Total length packed: 12.0cm
Container has one Ta heat shield.
No endcaps inserted to allow outgassing
Two TaC coated Ta wires formed into a spring inserted either end to avoid ZrC expansion of materials.
Currently being pumped down.
Friday, June 26, 2015, 11:44
HS water valves opened.
No leaks detected.
Initiating ramp up.
Friday, June 26, 2015, 14:44
EVAP2 was tapped up manually to 50A.
Vacuum tripped evap off.
Tapping back up manually now...
Friday, June 26, 2015, 15:53
Tapped up manually to 45A for both TGHT and TBHT
IGP1 = 4.8e-5 Torr
Will initiate auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively once vacuum settled down and stable.
Max setpoints set to 520A and 230A for the TGHT and TBHT respectively.
Good Vacuum = 3.0e-5 Torr. Bad Vacuum = 4.0e-5 Torr.
|
Monday, June 29, 2015, 07:05, John Wong, ZrC, 41177-2, LP-SIS, Done, Sintering back-up ZrC
|
Laura Lambert wrote: |
Thursday, June 25, 2015, 16:14
Total number of foils: 422 discs
Total mass of materials [incl graphite foils]:
Total length packed: 13.2cm
Container has one Ta heat shield.
No endcaps inserted to allow outgassing
Two TaC coated Ta wires formed into a spring inserted either end to avoid ZrC expansion of materials.
Currently being pumped down.
Friday, June 26, 2015, 11:44
HS water valves opened.
No leaks detected.
Initiating ramp up.
Friday, June 26, 2015, 14:44
EVAP2 was tapped up manually to 50A.
Vacuum tripped evap off.
Tapping back up manually now...
Friday, June 26, 2015, 15:53
Tapped up manually to 45A for both TGHT and TBHT
IGP1 = 4.8e-5 Torr
Will initiate auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively once vacuum settled down and stable.
Max setpoints set to 520A and 230A for the TGHT and TBHT respectively.
Good Vacuum = 3.0e-5 Torr. Bad Vacuum = 4.0e-5 Torr.
|
Monday, June 29, 2015, 06:57
TGHT has been at 520A/9.80V, DV 5.80V for 7 hours, temperature measured at 1800C. Vac is coming down to 9.18e-6 Torr. However, TGHT voltage is slightly going up over the 7 hours of heating, See screenshot attachment. (Can't make further comments until target is inspected.)
Initiated cooling down at 2A/min for TGHT and 1A/min for TBHT.
Chamber can be vented later today.
Monday, June 29, 2015, 14:58
Target has been inspected.
Slightly crystallization on the outer tube of the container can be observed.
Overall, the container looks a lot better than before.
Rn foiled inserted. Salt added - Ready for test-stand
|
Tuesday, June 23, 2015, 12:26, John Wong, SiC, 38817-6, HP-SIS, In progress, RUSH! SiC backup target undergoes sintering process
|
Tuesday, June 23, 2015, 12:21
Target container is loaded with 485 discs of SiC with packed length of 17.4cm.
Container is wrapped with 3 Ta-heat shields and previously coated/sintered with TaC.
Chamber is currently being pumped down
TGHT will be ramped up to 800A, ~1800C, and TBHT is limited to 230A max.
Tuesday, June 23, 2015, 15:53
HS valves are open, no leaks detected.
TGHT stepped up to 70A, pressure is currently at 4.17e-5 torr and coming up.
Initiated auto-ramping at 0.5A/min for both TGHT and TBHT: good vac at 3.0e-5, bad vac at 4.0e-5 Torr.
Wednesday, June 24, 2015, 00:03
Stopped auto-ramping about 2 hours ago.
Manual stepped up TGHT to 73A. Vac is stabilizing at 5e-8 Torr. Will keep it at that current over night.
Wednesday, June 24, 2015, 07:41
Vac has come down to 3.6e-6 Torr.
Continue to step up TGHT...
Wednesday, June 24, 2015, 23:52
It has been a super long day operating the evaporator and finally the target is up to 1800C. Vac is coming down from 2.e-5 Torr.
TGHT is at 790A/12.61V, DV at 6.60V, TBHT at 230A/3.57V. Omega temp reader is at 1680C - that's due to the window being coated with SiC, as expected.
Target will continue heated at that current for over night, and will start the cooling process next AM.
Thursday, June 25, 2015, 06:18
Target is holding pretty well over night. Vac is coming down to 1.6e-6 Torr.
Initiated cooling down at 2A/min.
|
Thursday, June 25, 2015, 16:13, Laura Lambert, SiC, 38817-6, HP-SIS, Done, RUSH! SiC backup target undergoes sintering process
|
John Wong wrote: |
Tuesday, June 23, 2015, 12:21
Target container is loaded with 485 discs of SiC with packed length of 17.4cm.
Container is wrapped with 3 Ta-heat shields and previously coated/sintered with TaC.
Chamber is currently being pumped down
TGHT will be ramped up to 800A, ~1800C, and TBHT is limited to 230A max.
Tuesday, June 23, 2015, 15:53
HS valves are open, no leaks detected.
TGHT stepped up to 70A, pressure is currently at 4.17e-5 torr and coming up.
Initiated auto-ramping at 0.5A/min for both TGHT and TBHT: good vac at 3.0e-5, bad vac at 4.0e-5 Torr.
Wednesday, June 24, 2015, 00:03
Stopped auto-ramping about 2 hours ago.
Manual stepped up TGHT to 73A. Vac is stabilizing at 5e-8 Torr. Will keep it at that current over night.
Wednesday, June 24, 2015, 07:41
Vac has come down to 3.6e-6 Torr.
Continue to step up TGHT...
Wednesday, June 24, 2015, 23:52
It has been a super long day operating the evaporator and finally the target is up to 1800C. Vac is coming down from 2.e-5 Torr.
TGHT is at 790A/12.61V, DV at 6.60V, TBHT at 230A/3.57V. Omega temp reader is at 1680C - that's due to the window being coated with SiC, as expected.
Target will continue heated at that current for over night, and will start the cooling process next AM.
Thursday, June 25, 2015, 06:18
Target is holding pretty well over night. Vac is coming down to 1.6e-6 Torr.
Initiated cooling down at 2A/min.
|
Thursday, June 25, 2015, 16:09
Vented in air and took out this afternoon.
Target looks good [see photos]
Window for OMEGA fully coated from outgassing of target materials |
Monday, June 22, 2015, 13:11, John Wong, Empty, 38817-6, HP-SIS, In progress, RUSH! Sintering TaC coated container for SiC
|
Monday, June 22, 2015, 13:00
Containers is coated with TaC. Wrapped with 3 layers of Ta heat-shield. Air blown to for quick dry.
Installed, and pumped down, vac currently at 6.7e-6 Torr.
HS water valve open, no leaks detected.
Stepping up TGHT/TBTH: 50A.
Monday, June 22, 2015, 14:22
Pressure is coming down, currently at 1.75e-5 Torr.
auto-ramping initiated: TGHT = 820A; TBHT = 230A, rate at 2A/min.
Tuesday, June 23, 2015, 00:50
Target container has reached to 1860C and has been heated for almost 4 hours, with TGHT at 800A/12.60V, DV = 6.28. TBHT at 230A/3.8V.
Vac at 3e-6 Torr.
Cooling down at 2A/min.
Chamber can be vented tomorrow and SiC can be loaded in for the sintering process.
|
Tuesday, June 23, 2015, 10:18, Laura Lambert, Empty, 38817-6, HP-SIS, Done, RUSH! Sintering TaC coated container for SiC
|
John Wong wrote: |
Monday, June 22, 2015, 13:00
Containers is coated with TaC. Wrapped with 3 layers of Ta heat-shield. Air blown to for quick dry.
Installed, and pumped down, vac currently at 6.7e-6 Torr.
HS water valve open, no leaks detected.
Stepping up TGHT/TBTH: 50A.
Monday, June 22, 2015, 14:22
Pressure is coming down, currently at 1.75e-5 Torr.
auto-ramping initiated: TGHT = 820A; TBHT = 230A, rate at 2A/min.
Tuesday, June 23, 2015, 00:50
Target container has reached to 1860C and has been heated for almost 4 hours, with TGHT at 800A/12.60V, DV = 6.28. TBHT at 230A/3.8V.
Vac at 3e-6 Torr.
Cooling down at 2A/min.
Chamber can be vented tomorrow and SiC can be loaded in for the sintering process.
|
Tuesday, June 23, 2015, 10:17
vented in air and opened up this morning.
coating looks good.
loading container now...
|
Thursday, June 18, 2015, 11:39, Rick Maharaj, , , , , Installation of Extraction Electrode Insulator - New Material
|
Tuesday June 16, 2015
An Extraction Insulator ITD0381 made from a different grade of AiN was installed in Evaporator 2 for testing purposes. The sub assembly included the SIS Restraint Housing ITD0389, New Extraction Insulator ITD0381, Repeller Electrode ITD0377, Extraction Electrode ITD0374 with fingerstock mounted.
The standoff insulator ITD0400 was found to be swelled up and broken. It was replaced with and glazed alumina insulator.
The tube heater Insulator ITD0342 - central support helicoil was repaired. |
Tuesday, June 09, 2015, 10:44, Laura Lambert, Empty, 41177-2, LP-SIS, In progress, Sintering TaC coating container for ZrC back-up
|
Tuesday, June 09, 2015, 9:16
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min.
TBHT will be ramped up to 230A at 01A/min.
Chamber is currently being pumped down.
Tuesday, June 09, 2015, 15:37
HS water valves were opened. no leaks detected.
Tapped up manually to 35A.
Once vacuum stabilized after ~45min, initiated auto-ramp.
Wednesday, June 10, 2015, 08:02
IGP1 = 5.3e-7 Torr.
TGHT = 250A and TBHT = 140A.
Increasing auto ramp to 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
|
Wednesday, June 10, 2015, 16:35, John Wong, Empty, 41177-2, LP-SIS, In progress, Sintering TaC coating container for ZrC back-up
|
Laura Lambert wrote: |
Tuesday, June 09, 2015, 9:16
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min.
TBHT will be ramped up to 230A at 01A/min.
Chamber is currently being pumped down.
Tuesday, June 09, 2015, 15:37
HS water valves were opened. no leaks detected.
Tapped up manually to 35A.
Once vacuum stabilized after ~45min, initiated auto-ramp.
Wednesday, June 10, 2015, 08:02
IGP1 = 5.3e-7 Torr.
TGHT = 250A and TBHT = 140A.
Increasing auto ramp to 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
|
Wednesday, June 10, 2015, 16:32
TGHT/TBHT are at 580A/230A for almost 6 hours, temp at 1728C.
Vac at 8.5e-7 Torr.
Cooling down initiated at 1A/min.
Target container should be inspected once the chamber is vented.
|
Thursday, June 11, 2015, 16:10, Laura Lambert, Empty, 41177-2, LP-SIS, In progress, Sintering TaC coating container for ZrC back-up
|
John Wong wrote: |
Laura Lambert wrote: |
Tuesday, June 09, 2015, 9:16
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min.
TBHT will be ramped up to 230A at 01A/min.
Chamber is currently being pumped down.
Tuesday, June 09, 2015, 15:37
HS water valves were opened. no leaks detected.
Tapped up manually to 35A.
Once vacuum stabilized after ~45min, initiated auto-ramp.
Wednesday, June 10, 2015, 08:02
IGP1 = 5.3e-7 Torr.
TGHT = 250A and TBHT = 140A.
Increasing auto ramp to 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
|
Wednesday, June 10, 2015, 16:32
TGHT/TBHT are at 580A/230A for almost 6 hours, temp at 1728C.
Vac at 8.5e-7 Torr.
Cooling down initiated at 1A/min.
Target container should be inspected once the chamber is vented.
|
Thursday, June 11, 2015, 10:55
Vented in air and opened up this morning.
Same as last container sintered in evap2 [IG-LIS for UCx#13] - ends not quite fully sintered and coating not very good.
most likely due to old TaC spray.
See link for photos.
https://www.dropbox.com/sh/75o43x8y2z16e7j/AABc8Z1fTTaTRtJ5_Jr1eacWa?dl=0
|
Monday, June 15, 2015, 15:30, John Wong, Empty, 41177-2, LP-SIS, Done, Re-Sintering TaC coating container for ZrC back-up
|
Laura Lambert wrote: |
John Wong wrote: |
Laura Lambert wrote: |
Tuesday, June 09, 2015, 9:16
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min.
TBHT will be ramped up to 230A at 01A/min.
Chamber is currently being pumped down.
Tuesday, June 09, 2015, 15:37
HS water valves were opened. no leaks detected.
Tapped up manually to 35A.
Once vacuum stabilized after ~45min, initiated auto-ramp.
Wednesday, June 10, 2015, 08:02
IGP1 = 5.3e-7 Torr.
TGHT = 250A and TBHT = 140A.
Increasing auto ramp to 2.0A/min and 1.0A/min for the TGHT and TBHT respectively.
|
Wednesday, June 10, 2015, 16:32
TGHT/TBHT are at 580A/230A for almost 6 hours, temp at 1728C.
Vac at 8.5e-7 Torr.
Cooling down initiated at 1A/min.
Target container should be inspected once the chamber is vented.
|
Thursday, June 11, 2015, 10:55
Vented in air and opened up this morning.
Same as last container sintered in evap2 [IG-LIS for UCx#13] - ends not quite fully sintered and coating not very good.
most likely due to old TaC spray.
See link for photos.
https://www.dropbox.com/sh/75o43x8y2z16e7j/AABc8Z1fTTaTRtJ5_Jr1eacWa?dl=0
|
Monday, June 15, 2015, 15:24
Same problem also found for the LP-IG-LIS container, WO#40860-1, see elog id#215. After re-coating and sintering, it seems better.
For this container, it is re-coated and will undergo the sintering process one more time.
Will try to go up to 1900C for the sintering process.
Target container is temporarily wrapped with 6.2cm of Ta foil as a layer for heat shield on each side of the tube, excluding the centre block. The shield will be removed once the process is done.
Target current will be controlled accordingly.
Chamber is being pumped down.
Monday, June 15, 2015, 16:17
HS water valves open; no leaks detected.
IGP1 at 6.8e-6 Torr and coming down.
Monday, June 15, 2015, 17:21
Stepping up TGHT/TBHT to 60A, pressure seems pretty stable at 7.2e-6 Torr and coming down.
Setting TGHT to 400A and TBHT to 230A, auto-ramping initiated. Will setup up current to reach 1900C, if necessary.
Monday, June 15, 2015, 20:28
TGHT and TBHT reached 400A/230A, Temp at 1552C. Vac at 2.7e-6 Torr.
Stepping TGHT
Monday, June 15, 2015, 21:16
TGHT at 520A/9.06 V to achieve 1900C. DV at 5.09V.
Vac at 4.2e-6 Torr.
Will continue the sintering process at this temperature for another 3-4 hours.
Tuesday, June 16, 2015, 00:15
Target container has been heated at 1900C for over 3 hours.
Vacuum is coming down to 1.4e-6 Torr.
Initiated cooling process at 2A/min
Chamber can be vented tomorrow and container should be inspected
Friday, June 26, 2015, 16:04
Container looks good!
|
Thursday, June 04, 2015, 11:10, Laura Lambert, Empty, , LP-IG-LIS, In progress, Sintering TaC coating container for UCx
|
Thursday, June 04, 2015, 9:07
Container was sprayed with TaC and let dry.
Container has 3x Ta heat shields including center block.
Container was loaded into EVAP2 yesterday and pumped down overnight.
HS water valves were opened up this morning, no leaks detected.
IGP1 = 4.6e-7 Torr.
Tapped up manually to 40A.
Waited ~25min, Vacuum stable.
IGP1 = 5.0e-7 Torr.
Initiating auto-ramp.
TGHT will be ramped to reach 2000C
Friday, June 05, 2015, 10:01
IGP1 = 4.5e-7 Torr.
TGHT = 313A, 4.47V
OMEGA = 1444C
Increasing ramping rate to 1.0A/min
Friday, June 05, 2015, 11:31
IGP1 = 1.2e-6 Torr.
Increasing ramping rate to 2.0A/min
|
Friday, June 05, 2015, 12:19, John Wong, Empty, , LP-IG-LIS, In progress, Sintering TaC coating container for UCx
|
Laura Lambert wrote: |
Thursday, June 04, 2015, 9:07
Container was sprayed with TaC and let dry.
Container has 3x Ta heat shields including center block.
Container was loaded into EVAP2 yesterday and pumped down overnight.
HS water valves were opened up this morning, no leaks detected.
IGP1 = 4.6e-7 Torr.
Tapped up manually to 40A.
Waited ~25min, Vacuum stable.
IGP1 = 5.0e-7 Torr.
Initiating auto-ramp.
TGHT will be ramped to reach 2000C
Friday, June 05, 2015, 10:01
IGP1 = 4.5e-7 Torr.
TGHT = 313A, 4.47V
OMEGA = 1444C
Increasing ramping rate to 1.0A/min
Friday, June 05, 2015, 11:31
IGP1 = 1.2e-6 Torr.
Increasing ramping rate to 2.0A/min
|
Friday, June 05, 2015, 12:01
TGHT reached to 465A/7.56V, temp is stable at 2000C. Current vac at 1.2e-6 Torr and coming down
Cooling down process can be initiated after 4 hours.
|
Friday, June 05, 2015, 13:22, Laura Lambert, Empty, 40860-1, LP-IG-LIS, In progress, Sintering TaC coating container for UCx
|
John Wong wrote: |
Laura Lambert wrote: |
Thursday, June 04, 2015, 9:07
Container was sprayed with TaC and let dry.
Container has 3x Ta heat shields including center block.
Container was loaded into EVAP2 yesterday and pumped down overnight.
HS water valves were opened up this morning, no leaks detected.
IGP1 = 4.6e-7 Torr.
Tapped up manually to 40A.
Waited ~25min, Vacuum stable.
IGP1 = 5.0e-7 Torr.
Initiating auto-ramp.
TGHT will be ramped to reach 2000C
Friday, June 05, 2015, 10:01
IGP1 = 4.5e-7 Torr.
TGHT = 313A, 4.47V
OMEGA = 1444C
Increasing ramping rate to 1.0A/min
Friday, June 05, 2015, 11:31
IGP1 = 1.2e-6 Torr.
Increasing ramping rate to 2.0A/min
|
Friday, June 05, 2015, 12:01
TGHT reached to 465A/7.56V, temp is stable at 2000C. Current vac at 1.2e-6 Torr and coming down
Cooling down process can be initiated after 4 hours.
|
Friday, June 05, 2015, 13:21
OMEGA = 1995C
Increasing TGHT to 470A to achieve desired max temperature of 2000C
Friday, June 05, 2015, 15:59
TGHT sat at max desired temperature of 2000C for ~4hrs.
TGHT = 470A, 7.7V
Initiating auto-cool at 1.0A/min.
Monday, June 08, 2015, 11:31
Vented in air and opened up this morning.
Target container mostly sintered, two tiny patches near both ends not fully sintered.
Will re-install and re-sinter next week as another container with priority needs to be sintered first.
Tuesday, June 09, 2015, 10:45
See attachements for 'not-fully-sintered' photos
|
Wednesday, June 10, 2015, 12:15, John Wong, Empty, 40860-1, LP-IG-LIS, In progress, Sintering TaC coating container for UCx
|
Laura Lambert wrote: |
John Wong wrote: |
Laura Lambert wrote: |
Thursday, June 04, 2015, 9:07
Container was sprayed with TaC and let dry.
Container has 3x Ta heat shields including center block.
Container was loaded into EVAP2 yesterday and pumped down overnight.
HS water valves were opened up this morning, no leaks detected.
IGP1 = 4.6e-7 Torr.
Tapped up manually to 40A.
Waited ~25min, Vacuum stable.
IGP1 = 5.0e-7 Torr.
Initiating auto-ramp.
TGHT will be ramped to reach 2000C
Friday, June 05, 2015, 10:01
IGP1 = 4.5e-7 Torr.
TGHT = 313A, 4.47V
OMEGA = 1444C
Increasing ramping rate to 1.0A/min
Friday, June 05, 2015, 11:31
IGP1 = 1.2e-6 Torr.
Increasing ramping rate to 2.0A/min
|
Friday, June 05, 2015, 12:01
TGHT reached to 465A/7.56V, temp is stable at 2000C. Current vac at 1.2e-6 Torr and coming down
Cooling down process can be initiated after 4 hours.
|
Friday, June 05, 2015, 13:21
OMEGA = 1995C
Increasing TGHT to 470A to achieve desired max temperature of 2000C
Friday, June 05, 2015, 15:59
TGHT sat at max desired temperature of 2000C for ~4hrs.
TGHT = 470A, 7.7V
Initiating auto-cool at 1.0A/min.
Monday, June 08, 2015, 11:31
Vented in air and opened up this morning.
Target container mostly sintered, two tiny patches near both ends not fully sintered.
Will re-install and re-sinter next week as another container with priority needs to be sintered first.
Tuesday, June 09, 2015, 10:45
See attachements for 'not-fully-sintered' photos
|
Wednesday, June 10, 2015, 12:06
After inspecting the target container, the inner tube surface has "dark" patches, which may not be evenly coated or the coating layer was too think.
See link for photos: https://www.dropbox.com/sh/m94mjuuodwhz5jb/AADEBv_Kha_p_1An40eftWNHa?dl=0
Attempt to re-spray the container and re-sinter.
|
Friday, June 12, 2015, 14:59, Laura Lambert, Empty, 40860-1, LP-IG-LIS, In progress, Sintering TaC coating container for UCx
|
John Wong wrote: |
Laura Lambert wrote: |
John Wong wrote: |
Laura Lambert wrote: |
Thursday, June 04, 2015, 9:07
Container was sprayed with TaC and let dry.
Container has 3x Ta heat shields including center block.
Container was loaded into EVAP2 yesterday and pumped down overnight.
HS water valves were opened up this morning, no leaks detected.
IGP1 = 4.6e-7 Torr.
Tapped up manually to 40A.
Waited ~25min, Vacuum stable.
IGP1 = 5.0e-7 Torr.
Initiating auto-ramp.
TGHT will be ramped to reach 2000C
Friday, June 05, 2015, 10:01
IGP1 = 4.5e-7 Torr.
TGHT = 313A, 4.47V
OMEGA = 1444C
Increasing ramping rate to 1.0A/min
Friday, June 05, 2015, 11:31
IGP1 = 1.2e-6 Torr.
Increasing ramping rate to 2.0A/min
|
Friday, June 05, 2015, 12:01
TGHT reached to 465A/7.56V, temp is stable at 2000C. Current vac at 1.2e-6 Torr and coming down
Cooling down process can be initiated after 4 hours.
|
Friday, June 05, 2015, 13:21
OMEGA = 1995C
Increasing TGHT to 470A to achieve desired max temperature of 2000C
Friday, June 05, 2015, 15:59
TGHT sat at max desired temperature of 2000C for ~4hrs.
TGHT = 470A, 7.7V
Initiating auto-cool at 1.0A/min.
Monday, June 08, 2015, 11:31
Vented in air and opened up this morning.
Target container mostly sintered, two tiny patches near both ends not fully sintered.
Will re-install and re-sinter next week as another container with priority needs to be sintered first.
Tuesday, June 09, 2015, 10:45
See attachements for 'not-fully-sintered' photos
|
Wednesday, June 10, 2015, 12:06
After inspecting the target container, the inner tube surface has "dark" patches, which may not be evenly coated or the coating layer was too think.
See link for photos: https://www.dropbox.com/sh/m94mjuuodwhz5jb/AADEBv_Kha_p_1An40eftWNHa?dl=0
Attempt to re-spray the container and re-sinter.
|
Friday, June 12, 2015, 14:58
re-sprayed with second layer of TaC spray this morning.
re-loaded into evap2.
HS water valves opened, no leaks detected.
will ramp-up over weekend. |
Friday, June 12, 2015, 16:08, John Wong, Empty, 40860-1, LP-IG-LIS, In progress, Re-Sintering TaC coating container for UCx
|
Laura Lambert wrote: |
John Wong wrote: |
Laura Lambert wrote: |
John Wong wrote: |
Laura Lambert wrote: |
Thursday, June 04, 2015, 9:07
Container was sprayed with TaC and let dry.
Container has 3x Ta heat shields including center block.
Container was loaded into EVAP2 yesterday and pumped down overnight.
HS water valves were opened up this morning, no leaks detected.
IGP1 = 4.6e-7 Torr.
Tapped up manually to 40A.
Waited ~25min, Vacuum stable.
IGP1 = 5.0e-7 Torr.
Initiating auto-ramp.
TGHT will be ramped to reach 2000C
Friday, June 05, 2015, 10:01
IGP1 = 4.5e-7 Torr.
TGHT = 313A, 4.47V
OMEGA = 1444C
Increasing ramping rate to 1.0A/min
Friday, June 05, 2015, 11:31
IGP1 = 1.2e-6 Torr.
Increasing ramping rate to 2.0A/min
|
Friday, June 05, 2015, 12:01
TGHT reached to 465A/7.56V, temp is stable at 2000C. Current vac at 1.2e-6 Torr and coming down
Cooling down process can be initiated after 4 hours.
|
Friday, June 05, 2015, 13:21
OMEGA = 1995C
Increasing TGHT to 470A to achieve desired max temperature of 2000C
Friday, June 05, 2015, 15:59
TGHT sat at max desired temperature of 2000C for ~4hrs.
TGHT = 470A, 7.7V
Initiating auto-cool at 1.0A/min.
Monday, June 08, 2015, 11:31
Vented in air and opened up this morning.
Target container mostly sintered, two tiny patches near both ends not fully sintered.
Will re-install and re-sinter next week as another container with priority needs to be sintered first.
Tuesday, June 09, 2015, 10:45
See attachements for 'not-fully-sintered' photos
|
Wednesday, June 10, 2015, 12:06
After inspecting the target container, the inner tube surface has "dark" patches, which may not be evenly coated or the coating layer was too think.
See link for photos: https://www.dropbox.com/sh/m94mjuuodwhz5jb/AADEBv_Kha_p_1An40eftWNHa?dl=0
Attempt to re-spray the container and re-sinter.
|
Friday, June 12, 2015, 14:58
re-sprayed with second layer of TaC spray this morning.
re-loaded into evap2.
HS water valves opened, no leaks detected.
will ramp-up over weekend.
|
Friday, June 12, 2015, 16:07
Vacuum comes down to 6.1e-6 Torr.
Initiated auto-ramping at 0.2A/min for 300A first.
|
Sunday, June 14, 2015, 09:40, John Wong, Empty, 40860-1, LP-IG-LIS, Done, Re-Sintering TaC coating container for UCx
|
John Wong wrote: |
Laura Lambert wrote: |
John Wong wrote: |
Laura Lambert wrote: |
John Wong wrote: |
Laura Lambert wrote: |
Thursday, June 04, 2015, 9:07
Container was sprayed with TaC and let dry.
Container has 3x Ta heat shields including center block.
Container was loaded into EVAP2 yesterday and pumped down overnight.
HS water valves were opened up this morning, no leaks detected.
IGP1 = 4.6e-7 Torr.
Tapped up manually to 40A.
Waited ~25min, Vacuum stable.
IGP1 = 5.0e-7 Torr.
Initiating auto-ramp.
TGHT will be ramped to reach 2000C
Friday, June 05, 2015, 10:01
IGP1 = 4.5e-7 Torr.
TGHT = 313A, 4.47V
OMEGA = 1444C
Increasing ramping rate to 1.0A/min
Friday, June 05, 2015, 11:31
IGP1 = 1.2e-6 Torr.
Increasing ramping rate to 2.0A/min
|
Friday, June 05, 2015, 12:01
TGHT reached to 465A/7.56V, temp is stable at 2000C. Current vac at 1.2e-6 Torr and coming down
Cooling down process can be initiated after 4 hours.
|
Friday, June 05, 2015, 13:21
OMEGA = 1995C
Increasing TGHT to 470A to achieve desired max temperature of 2000C
Friday, June 05, 2015, 15:59
TGHT sat at max desired temperature of 2000C for ~4hrs.
TGHT = 470A, 7.7V
Initiating auto-cool at 1.0A/min.
Monday, June 08, 2015, 11:31
Vented in air and opened up this morning.
Target container mostly sintered, two tiny patches near both ends not fully sintered.
Will re-install and re-sinter next week as another container with priority needs to be sintered first.
Tuesday, June 09, 2015, 10:45
See attachements for 'not-fully-sintered' photos
|
Wednesday, June 10, 2015, 12:06
After inspecting the target container, the inner tube surface has "dark" patches, which may not be evenly coated or the coating layer was too think.
See link for photos: https://www.dropbox.com/sh/m94mjuuodwhz5jb/AADEBv_Kha_p_1An40eftWNHa?dl=0
Attempt to re-spray the container and re-sinter.
|
Friday, June 12, 2015, 14:58
re-sprayed with second layer of TaC spray this morning.
re-loaded into evap2.
HS water valves opened, no leaks detected.
will ramp-up over weekend.
|
Friday, June 12, 2015, 16:07
Vacuum comes down to 6.1e-6 Torr.
Initiated auto-ramping at 0.2A/min for 300A first.
|
Sunday, June 14, 2015, 09:37
TGHT at 254.2A/3.5V3, DV = 1.614V Temp at 1177C.
Vacuum is stable at 3.2e-7 Torr.
Increase ramping rate at 2A/min until TGHT reached 300A.
Sunday, June 14, 2015, 10:04
TGHT reached 300A, temp 1368C.
Tapping up to ~1800C
Sunday, June 14, 2015, 11:26
TGHT at 425A/6.84V, DV 3.59V, temp at 1814C,
Vacuum coming down, currently at 7.5e-7 Torr.
Will remain at that current for at least 4 hours before cooling down
Sunday, June 14, 2015, 17:15
Target container has been sintered with TiC for over 6 hours at 1823C, with TGHT at 425A/6.84V, DV at 3.584V.
Vac at 4.9e-7 Torr.
Cooling initiated.
Chamber can be vented tomorrow and target container can be taken out for inspection.
Monday, June 15, 2015, 11:38
Target container was taken out for inspection.
It's observed that the coated/sintered TaC surface is improved. The sintered temperature was only gone up just above 1800C, so there still some area near the ends that is still somewhat "brownish", fully sintered shows a
smooth . (see attachment)
Spraying into a cylinder tube can be challenging. It was observed that the coating was dispersed out from the end cap to the centre tube. For that reason, the container isn't has much protective layer;vthe Ta surface can
react with carbides and the container eventually breaks. Take the endcap process for example, the caps are evenly coated with TaC and can be sintered up to 2000C (see e-log Evap ID 202).
Suggestions:
Using a spray ball nozzle or some sort so that the inner tube can be evenly coated.
Under investigating...
|
Friday, May 29, 2015, 11:29, Laura Lambert, ZrC, 41177-1, LP-SIS, In progress, Conditioning ZrC#7
|
Friday, May 29, 2015, 11:21
Total number of foils: 425 discs
Total mass of materials [incl graphite foils]: 44.41g
Total length packed: 12.3cm
Container has no heat shields.
No endcaps inserted to allow outgassing.
Currently being pumped down.
Friday, May 29, 2015, 14:13
HS water valves opened, no leaks detected.
IGP1 = 5.4e-6 Torr.
Tapping up manually.
Friday, May 29, 2015, 16:48
Tapped up manually to 20A.
IGP1 = 5.9e-6 Torr.
Initiating auto-ramp at 0.2A/min for the TGHT and 0.1A/min for the TBHT.
Max setpoints set to 580A and 230A for the TGHT and TBHT respectively.
Good Vacuum = 3.0e-5 Torr. Bad Vacuum = 4.0e-5 Torr.
Monday, June 01, 2015, 09:17
IGP1 = 3.8e-6 Torr.
TGHT = 478A.
TBHT reached max setpoint of 230A.
Increasing ramping rate to 0.5A/min.
Monday, June 01, 2015, 13:15
Checked window for temperature readings, good visibility, no coating on window.
IGP1 = 9.1e-6 Torr.
TGHT reached max setpoint of 580A 30min ago.
Stepping up manually to a target temperature of 2000C...
Monday, June 01, 2015, 16:25
IGP1 = 6.5e-6 Torr.
TGHT = 870A, 17.90V
OMEGA = 1948C
|
Monday, June 01, 2015, 18:09, John Wong, ZrC, 41177-1, LP-SIS, In progress, Conditioning ZrC#7
|
Laura Lambert wrote: |
Friday, May 29, 2015, 11:21
Total number of foils: 425 discs
Total mass of materials [incl graphite foils]: 44.41g
Total length packed: 12.3cm
Container has no heat shields.
No endcaps inserted to allow outgassing.
Currently being pumped down.
Friday, May 29, 2015, 14:13
HS water valves opened, no leaks detected.
IGP1 = 5.4e-6 Torr.
Tapping up manually.
Friday, May 29, 2015, 16:48
Tapped up manually to 20A.
IGP1 = 5.9e-6 Torr.
Initiating auto-ramp at 0.2A/min for the TGHT and 0.1A/min for the TBHT.
Max setpoints set to 580A and 230A for the TGHT and TBHT respectively.
Good Vacuum = 3.0e-5 Torr. Bad Vacuum = 4.0e-5 Torr.
Monday, June 01, 2015, 09:17
IGP1 = 3.8e-6 Torr.
TGHT = 478A.
TBHT reached max setpoint of 230A.
Increasing ramping rate to 0.5A/min.
Monday, June 01, 2015, 13:15
Checked window for temperature readings, good visibility, no coating on window.
IGP1 = 9.1e-6 Torr.
TGHT reached max setpoint of 580A 30min ago.
Stepping up manually to a target temperature of 2000C...
Monday, June 01, 2015, 16:25
IGP1 = 6.5e-6 Torr.
TGHT = 870A, 17.90V
OMEGA = 1948C
|
Monday, June 01, 2015, 17:59
After almost an hour at 870A, the temperature went up from 1948C to 1980C; however temperature around the target container/legs are >2000C. The voltage on the power supply also went up slightly.
There is a film coated on the window port and that could affect the temp reading.
To be safe, I lowered the TGHT to 830A/17.38V, temp at 1930C.
Will keep at 830A for 4 hours and cool down this evening.
Recommend: Using Ta-heat shields for sintering next time.
Monday, June 01, 2015, 22:55
TGHT at 830A for almost 5 hours.
TEMP has gone up to 1994C. Voltage has also gone up to 19V.
Cooling down at 2A/min for TGHT and 1A/min for TBHT.
|
Tuesday, June 02, 2015, 13:05, John Wong, ZrC, 41177-1, LP-SIS, Done, Conditioning ZrC#7
|
John Wong wrote: |
Laura Lambert wrote: |
Friday, May 29, 2015, 11:21
Total number of foils: 425 discs
Total mass of materials [incl graphite foils]: 44.41g
Total length packed: 12.3cm
Container has no heat shields.
No endcaps inserted to allow outgassing.
Currently being pumped down.
Friday, May 29, 2015, 14:13
HS water valves opened, no leaks detected.
IGP1 = 5.4e-6 Torr.
Tapping up manually.
Friday, May 29, 2015, 16:48
Tapped up manually to 20A.
IGP1 = 5.9e-6 Torr.
Initiating auto-ramp at 0.2A/min for the TGHT and 0.1A/min for the TBHT.
Max setpoints set to 580A and 230A for the TGHT and TBHT respectively.
Good Vacuum = 3.0e-5 Torr. Bad Vacuum = 4.0e-5 Torr.
Monday, June 01, 2015, 09:17
IGP1 = 3.8e-6 Torr.
TGHT = 478A.
TBHT reached max setpoint of 230A.
Increasing ramping rate to 0.5A/min.
Monday, June 01, 2015, 13:15
Checked window for temperature readings, good visibility, no coating on window.
IGP1 = 9.1e-6 Torr.
TGHT reached max setpoint of 580A 30min ago.
Stepping up manually to a target temperature of 2000C...
Monday, June 01, 2015, 16:25
IGP1 = 6.5e-6 Torr.
TGHT = 870A, 17.90V
OMEGA = 1948C
|
Monday, June 01, 2015, 17:59
After almost an hour at 870A, the temperature went up from 1948C to 1980C; however temperature around the target container/legs are >2000C. The voltage on the power supply also went up slightly.
There is a film coated on the window port and that could affect the temp reading.
To be safe, I lowered the TGHT to 830A/17.38V, temp at 1930C.
Will keep at 830A for 4 hours and cool down this evening.
Recommend: Using Ta-heat shields for sintering next time.
Monday, June 01, 2015, 22:55
TGHT at 830A for almost 5 hours.
TEMP has gone up to 1994C. Voltage has also gone up to 19V.
Cooling down at 2A/min for TGHT and 1A/min for TBHT.
|
Tuesday, June 02, 2015, 12:37
Chamber was vented and the target was inspected.
Some stressed marks on the target container can be observed.
The container is also slightly curved but otherwise it's fine.
The materials packed length has expended outward so 3 discs were removed in order to insert the end caps.
The packed length is now 16cm.
Two extra graphite foils were inserted on both ends, and previously coated/sintered TaC-end caps are inserted and expended.
Rn foil is inserted & Std solutions are added.
Ready for test-stand.
Link to photos for more details:
https://www.dropbox.com/sh/0cra7viqs9ro8q3/AADEGk8goGI4c-uzRQSGwWmxa?dl=0
|
Wednesday, June 03, 2015, 10:47, Laura Lambert, ZrC, 41177-1, LP-SIS, Done, Conditioning ZrC#7
|
John Wong wrote: |
John Wong wrote: |
Laura Lambert wrote: |
Friday, May 29, 2015, 11:21
Total number of foils: 425 discs
Total mass of materials [incl graphite foils]: 44.41g
Total length packed: 12.3cm
Container has no heat shields.
No endcaps inserted to allow outgassing.
Currently being pumped down.
Friday, May 29, 2015, 14:13
HS water valves opened, no leaks detected.
IGP1 = 5.4e-6 Torr.
Tapping up manually.
Friday, May 29, 2015, 16:48
Tapped up manually to 20A.
IGP1 = 5.9e-6 Torr.
Initiating auto-ramp at 0.2A/min for the TGHT and 0.1A/min for the TBHT.
Max setpoints set to 580A and 230A for the TGHT and TBHT respectively.
Good Vacuum = 3.0e-5 Torr. Bad Vacuum = 4.0e-5 Torr.
Monday, June 01, 2015, 09:17
IGP1 = 3.8e-6 Torr.
TGHT = 478A.
TBHT reached max setpoint of 230A.
Increasing ramping rate to 0.5A/min.
Monday, June 01, 2015, 13:15
Checked window for temperature readings, good visibility, no coating on window.
IGP1 = 9.1e-6 Torr.
TGHT reached max setpoint of 580A 30min ago.
Stepping up manually to a target temperature of 2000C...
Monday, June 01, 2015, 16:25
IGP1 = 6.5e-6 Torr.
TGHT = 870A, 17.90V
OMEGA = 1948C
|
Monday, June 01, 2015, 17:59
After almost an hour at 870A, the temperature went up from 1948C to 1980C; however temperature around the target container/legs are >2000C. The voltage on the power supply also went up slightly.
There is a film coated on the window port and that could affect the temp reading.
To be safe, I lowered the TGHT to 830A/17.38V, temp at 1930C.
Will keep at 830A for 4 hours and cool down this evening.
Recommend: Using Ta-heat shields for sintering next time.
Monday, June 01, 2015, 22:55
TGHT at 830A for almost 5 hours.
TEMP has gone up to 1994C. Voltage has also gone up to 19V.
Cooling down at 2A/min for TGHT and 1A/min for TBHT.
|
Tuesday, June 02, 2015, 12:37
Chamber was vented and the target was inspected.
Some stressed marks on the target container can be observed.
The container is also slightly curved but otherwise it's fine.
The materials packed length has expended outward so 3 discs were removed in order to insert the end caps.
The packed length is now 16cm.
Two extra graphite foils were inserted on both ends, and previously coated/sintered TaC-end caps are inserted and expended.
Rn foil is inserted & Std solutions are added.
Ready for test-stand.
Link to photos for more details:
https://www.dropbox.com/sh/0cra7viqs9ro8q3/AADEGk8goGI4c-uzRQSGwWmxa?dl=0
|
see attachment for data recorded during ZrC conditioning |
Thursday, May 28, 2015, 11:36, Laura Lambert, Endcaps, 40282-5, TARGET BOAT, In progress, Sintering TaC coating on Ta endcaps - round 2
|
Thursday, May 28, 2015, 11:34
Endcaps were sintered [see elog#199]
A Ta foil is placed in the target boat with separate slots for each endcap [see image]
The target boat is wrapped with 3-layers of Ta-heat shield.
The boat is installed in EVAP2, chamber is currently being pumped down.
Thursday, May 28, 2015, 14:01
HS water valves opened, no leaks detected.
IGP1 = 1.4e-6 Torr.
Initiating manual tap up.
Thursday, May 28, 2015, 15:10
Manually tapped up TGHT to 108A, 1.1V
Initiating auto-ramp at 2.0A/min with a max setpoint of 300A
Thursday, May 28, 2015, 15:22
Hoping to speed up the process...
IGP1 = 1.0e-6 Torr.
Increasing ramping rate to 4.0A/min with a max setpoint of 500A
Final desired temperature = 1800C
|
Thursday, May 28, 2015, 17:50, John Wong, Endcaps, 40282-5, TARGET BOAT, Done, Sintering TaC coating on Ta endcaps - round 2
|
Laura Lambert wrote: |
Thursday, May 28, 2015, 11:34
Endcaps were sintered [see elog#199]
A Ta foil is placed in the target boat with separate slots for each endcap [see image]
The target boat is wrapped with 3-layers of Ta-heat shield.
The boat is installed in EVAP2, chamber is currently being pumped down.
Thursday, May 28, 2015, 14:01
HS water valves opened, no leaks detected.
IGP1 = 1.4e-6 Torr.
Initiating manual tap up.
Thursday, May 28, 2015, 15:10
Manually tapped up TGHT to 108A, 1.1V
Initiating auto-ramp at 2.0A/min with a max setpoint of 300A
Thursday, May 28, 2015, 15:22
Hoping to speed up the process...
IGP1 = 1.0e-6 Torr.
Increasing ramping rate to 4.0A/min with a max setpoint of 500A
Final desired temperature = 1800C
|
Thursday, May 28, 2015, 17:42
TGHT at 500A. Temp at 1780C.
Increased TGHT to 580A (online operating current), Temp 1945C, vac 2.9e-6 torr and coming down. Will remain at that current for the sintering process.
Cooling it down later this evening.
Thursday, May 28, 2015, 21:27
Temp stabilized at 1960C with TGHT at 580A for almost 4 hours. Vacuum at 1.8e-7 Torr.
Cooling down initiated at 2A/min.
|
Friday, May 29, 2015, 11:18, Laura Lambert, Endcaps, 40282-5, TARGET BOAT, Done, Sintering TaC coating on Ta endcaps - round 2
|
John Wong wrote: |
Laura Lambert wrote: |
Thursday, May 28, 2015, 11:34
Endcaps were sintered [see elog#199]
A Ta foil is placed in the target boat with separate slots for each endcap [see image]
The target boat is wrapped with 3-layers of Ta-heat shield.
The boat is installed in EVAP2, chamber is currently being pumped down.
Thursday, May 28, 2015, 14:01
HS water valves opened, no leaks detected.
IGP1 = 1.4e-6 Torr.
Initiating manual tap up.
Thursday, May 28, 2015, 15:10
Manually tapped up TGHT to 108A, 1.1V
Initiating auto-ramp at 2.0A/min with a max setpoint of 300A
Thursday, May 28, 2015, 15:22
Hoping to speed up the process...
IGP1 = 1.0e-6 Torr.
Increasing ramping rate to 4.0A/min with a max setpoint of 500A
Final desired temperature = 1800C
|
Thursday, May 28, 2015, 17:42
TGHT at 500A. Temp at 1780C.
Increased TGHT to 580A (online operating current), Temp 1945C, vac 2.9e-6 torr and coming down. Will remain at that current for the sintering process.
Cooling it down later this evening.
Thursday, May 28, 2015, 21:27
Temp stabilized at 1960C with TGHT at 580A for almost 4 hours. Vacuum at 1.8e-7 Torr.
Cooling down initiated at 2A/min.
|
Friday, May 29, 2015, 11:16
Vented in air and opened up this morning.
Endcaps look great!
Sintering was spot on [see pictures]
|
Tuesday, May 26, 2015, 13:57, Laura Lambert, Endcaps, 40282-5, TARGET BOAT, In progress, Sintering TaC coating on Ta endcaps
|
Tuesday, May 26, 2015, 13:06
Endcaps were sprayed with TaC coating and let dry.
Each endcap is wrapped separately with a sheet of graphite foil and stacked in the target boat [see image]
The target boat is wrapped with 3-layers of Ta-heat shield.
The boat is installed in EVAP2, chamber is currently being pumped down.
Wednesday, May 27, 2015, 08:50
HS water valves opened, no leaks detected.
Stepped up manually to 35A.
Initiated auto-ramp at 0.2A/min yesterday afternoon.
TGHT = 254A, 3.56V.
IGP1 = 5.9e-7 Torr.
Increasing ramping rate to 1.0A/min with a max setpoint of 400A.
|
Wednesday, May 27, 2015, 17:58, John Wong, Endcaps, 40282-5, TARGET BOAT, In progress, Sintering TaC coating on Ta endcaps
|
Laura Lambert wrote: |
Tuesday, May 26, 2015, 13:06
Endcaps were sprayed with TaC coating and let dry.
Each endcap is wrapped separately with a sheet of graphite foil and stacked in the target boat [see image]
The target boat is wrapped with 3-layers of Ta-heat shield.
The boat is installed in EVAP2, chamber is currently being pumped down.
Wednesday, May 27, 2015, 08:50
HS water valves opened, no leaks detected.
Stepped up manually to 35A.
Initiated auto-ramp at 0.2A/min yesterday afternoon.
TGHT = 254A, 3.56V.
IGP1 = 5.9e-7 Torr.
Increasing ramping rate to 1.0A/min with a max setpoint of 400A.
|
Wednesday, May 27, 2015, 17:51
TGHT has been at 400A for almost 6 hours. Temp at 1500C.
Cooling down to 0A at 1A/min.
Chamber will be vented to inspect the caps.
May have to remove the graphite foil wrapped on the caps and re-sintered the caps to 1800C.
|
Thursday, May 28, 2015, 10:23, Laura Lambert, Endcaps, 40282-5, TARGET BOAT, Problems, Sintering TaC coating on Ta endcaps - not fully sintered
|
John Wong wrote: |
Laura Lambert wrote: |
Tuesday, May 26, 2015, 13:06
Endcaps were sprayed with TaC coating and let dry.
Each endcap is wrapped separately with a sheet of graphite foil and stacked in the target boat [see image]
The target boat is wrapped with 3-layers of Ta-heat shield.
The boat is installed in EVAP2, chamber is currently being pumped down.
Wednesday, May 27, 2015, 08:50
HS water valves opened, no leaks detected.
Stepped up manually to 35A.
Initiated auto-ramp at 0.2A/min yesterday afternoon.
TGHT = 254A, 3.56V.
IGP1 = 5.9e-7 Torr.
Increasing ramping rate to 1.0A/min with a max setpoint of 400A.
|
Wednesday, May 27, 2015, 17:51
TGHT has been at 400A for almost 6 hours. Temp at 1500C.
Cooling down to 0A at 1A/min.
Chamber will be vented to inspect the caps.
May have to remove the graphite foil wrapped on the caps and re-sintered the caps to 1800C.
|
Thursday, May 28, 2015, 08:13
Vented in air and opened up this morning.
Not fully sintered [see pictures]
|
Friday, May 22, 2015, 11:44, Laura Lambert, Empty, , TARGET BOAT, In progress, Sintering TaC coating on Ta target boat
|
Friday, May 22, 2015, 11:43
A target boat was sprayed with TaC coating and let dry yesterday.
The target boat is wrapped with 3-layers of Ta-heat shield.
The boat was installed in EVAP2, chamber is currently being pumped down.
Friday, May 22, 2015, 14:22
HS water valves opened, no leaks detected.
IGP1 = 2.4e-6 Torr.
Tapping up manually...
Friday, May 22, 2015, 14:33
Tapped up to 20A.
Vacuum jumped up to 7e-6 Torr.
Backed off to 5A before vacuum started to drop again.
IGP1 = 5e-6 Torr.
Tapping up manually again...just more slowly...
Friday, May 22, 2015, 15:31
Tapped up to 12A, unable to tap up very fast due to volatile content in coating.
IGP1 = 3.6e-6 Torr.
Initiating auto-ramp at 0.1A/min with a max current of 580A.
Monday, May 25, 2015, 09:03
IGP1 = 3e-7 Torr.
TGHT = 397.5A, 6.43V
Increasing ramping rate to 1.0A/min.
|
Monday, May 25, 2015, 17:08, John Wong, Empty, 40282-5, TARGET BOAT, In progress, Sintering TaC coating on Ta target boat
|
Laura Lambert wrote: |
Friday, May 22, 2015, 11:43
A target boat was sprayed with TaC coating and let dry yesterday.
The target boat is wrapped with 3-layers of Ta-heat shield.
The boat was installed in EVAP2, chamber is currently being pumped down.
Friday, May 22, 2015, 14:22
HS water valves opened, no leaks detected.
IGP1 = 2.4e-6 Torr.
Tapping up manually...
Friday, May 22, 2015, 14:33
Tapped up to 20A.
Vacuum jumped up to 7e-6 Torr.
Backed off to 5A before vacuum started to drop again.
IGP1 = 5e-6 Torr.
Tapping up manually again...just more slowly...
Friday, May 22, 2015, 15:31
Tapped up to 12A, unable to tap up very fast due to volatile content in coating.
IGP1 = 3.6e-6 Torr.
Initiating auto-ramp at 0.1A/min with a max current of 580A.
Monday, May 25, 2015, 09:03
IGP1 = 3e-7 Torr.
TGHT = 397.5A, 6.43V
Increasing ramping rate to 1.0A/min.
|
Monday, May 25, 2015, 17:06
TGHT at been at 580A for over 4 hours. Cooling down in process at 1A/min.
|
Tuesday, May 26, 2015, 13:05, Laura Lambert, Empty, 40282-5, TARGET BOAT, Done, Sintering TaC coating on Ta target boat
|
John Wong wrote: |
Laura Lambert wrote: |
Friday, May 22, 2015, 11:43
A target boat was sprayed with TaC coating and let dry yesterday.
The target boat is wrapped with 3-layers of Ta-heat shield.
The boat was installed in EVAP2, chamber is currently being pumped down.
Friday, May 22, 2015, 14:22
HS water valves opened, no leaks detected.
IGP1 = 2.4e-6 Torr.
Tapping up manually...
Friday, May 22, 2015, 14:33
Tapped up to 20A.
Vacuum jumped up to 7e-6 Torr.
Backed off to 5A before vacuum started to drop again.
IGP1 = 5e-6 Torr.
Tapping up manually again...just more slowly...
Friday, May 22, 2015, 15:31
Tapped up to 12A, unable to tap up very fast due to volatile content in coating.
IGP1 = 3.6e-6 Torr.
Initiating auto-ramp at 0.1A/min with a max current of 580A.
Monday, May 25, 2015, 09:03
IGP1 = 3e-7 Torr.
TGHT = 397.5A, 6.43V
Increasing ramping rate to 1.0A/min.
|
Monday, May 25, 2015, 17:06
TGHT at been at 580A for over 4 hours. Cooling down in process at 1A/min.
|
Vented in air and opened up this morning.
Target boat looks good! fully sintered! |
Tuesday, May 19, 2015, 13:54, Laura Lambert, Empty, 41177-1, LP-SIS, Done, Sintering TaC coating container for ZrC
|
Tuesday, May 19, 2015, 13:33
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min.
TBHT will be ramped up to 230A at 0.1A/min.
Chamber is currently being pumped down
Tuesday, May 19, 2015, 15:04
Opened up HS water, no leaks detected.
Stepped up to 35A.
Waited ~35min, vacuum stable.
IGP1 = 1.7e-6 Torr.
Initiating auto-ramp.
Wednesday, May 20, 2015, 11:43
IGP1 = 3e-7 Torr.
TGHT = 282A, 3.8V
TBHT = 156A, 2.2V
Increasing ramping rate to 1.0A/min and 0.5A/min for the TGHT and TBHT respectively.
Thursday, May 21, 2015, 10:42
IGP1 = 2.9e-7
Direct voltage = 5.48V
OMEGA = 1703C.
Initiating auto-cool at 2.0A/min and 1.0A/min for the TGHT and TBHT.
Friday, May 22, 2015, 11:41
Vented in air and opened up this morning.
TaC coating fully sintered, looks good!
|
Wednesday, May 13, 2015, 16:01, Laura Lambert, , 40282-4, TARGET BOAT, Done, Sintering three different ZrC samples
|
Wednesday, May 13, 2015, 15:21
Three different samples of ZrC are loaded into a target boat.
Sample A: ZrC + NO graphite
Sample B: ZrC + graphite [1:0.5 molar ratio]
Sample C: ZrC + graphite [1:1 molar ratio]
Each sample consists of 20 discs, stacked together and wrapped in graphite sheet
The target boat is wrapped with 3 x Ta heat shield.
EVAP2 pumping down overnight...
Thursday, May 14, 2015, 08:20
HS water valves opened up this a.m, no leaks detected.
IGP1 = 6.6e-7 Torr
Tapping up manually to 35A.
Good Vacuum = 3.00 e-5 Torr. Bad Vacuum = 4.00 e-5 Torr.
Thursday, May 14, 2015, 09:51
Tapped up manually to 30A.
After ~25min, vacuum gone up to IGP1 = 3.5e-5 Torr!
Backed off to 20A.
Waited ~10min. IGP1 = 1.75e-5 Torr.
Tapped back up to 25A.
Waited ~20min, IGP1 = 1.4e-5 Torr.
Tapped up to 30A.
Waited ~20min, IGP1 = 2.2e-5 Torr.
Tapped up to 35A
Waited ~50min, IGP1 = 2.5e-5 Torr.
Continuing manual tap-up...
Thursday, May 14, 2015, 13:27
IGP1 = 9e-6 Torr
Tapped up to 40A.
Waited ~45min, IGP1 = 1e-5 Torr
Initiating auto-ramp at 0.1A/min for the TGHT with a max setpoint of 275A/ 8.0V
Friday, May 15, 2015, 08:25
Max setpoints were changed to 400A/ 8.0V last night.
Reached 400A ~4.5hrs ago.
IGP1 = 4.9e-5 Torr
Initiating manual tap up and recording data.
Friday, May 15, 2015, 15:50
Samples remained at ~2000C for ~4 hours [see attachment for data]
IGP1 = 7.8e-7 Torr.
Initiating auto-cool at 1.0A/min.
Tuesday, May 19, 2015, 08:27
Vented in air and opened up this morning.
|
Friday, May 01, 2015, 10:50, Laura Lambert, , 40282-4, TARGET BOAT, In progress, Sintering four different ZrC samples
|
Friday, May 01, 2015, 10:27
Four different samples of ZrC are loaded into a target boat.
Sample A: ZrC + NO graphite / hand cut
Sample B: ZrC + NO graphite / laser cut
Sample C: ZrC + graphite / hand cut
Sample D: ZrC + graphite / laser cut
A picture showing the different samples is attached [one face-up/ one face-down sample of each side-by-side]
Each sample consists of ~20-25 discs, stacked together and wrapped in graphite sheet [see attachment for photo]
The target boat is wrapped with 3 x Ta heat shield.
EVAP1 pumped down overnight.
HS water valves were opened this morning, no leaks detected.
IGP1 = 5.5e-7 Torr.
Tapping up TGHT manually to 30A...
Friday, May 01, 2015, 10:54
Tapped up manually to 30A.
Over the course of 20min the vacuum climbed to IGP1 = 1.0 e-5 Torr.
Backed off TGHT to 20A to allow vacuum to stabilize.
Waited ~10min.
Vacuum dropped to IGP1 = 6.5e-6 Torr.
Tapped back-up manually to 30A.
Waited ~45min.
Vacuum stable, IGP1 = 1.2e-5 Torr.
Initiating auto-ramp at 0.1A/min for the TGHT with a max setpoint of 300A / 5.00V.
Good Vacuum = 3.00e-5 Torr. Bad vacuum = 4.00e-5 Torr.
Monday, May 04, 2015, 11:17
IGP1 = 2e-7 Torr.
TGHT = 274A, 4.75V
Ramp-up limited to 275A due to max voltage being set at 5.0V
Increased max voltage to 10V
Tapping up manually to 1800C and recording data.
|
Monday, May 04, 2015, 17:26, John Wong, , 40282-4, TARGET BOAT, In progress, Sintering four different ZrC samples
|
Laura Lambert wrote: |
Friday, May 01, 2015, 10:27
Four different samples of ZrC are loaded into a target boat.
Sample A: ZrC + NO graphite / hand cut
Sample B: ZrC + NO graphite / laser cut
Sample C: ZrC + graphite / hand cut
Sample D: ZrC + graphite / laser cut
A picture showing the different samples is attached [one face-up/ one face-down sample of each side-by-side]
Each sample consists of ~20-25 discs, stacked together and wrapped in graphite sheet [see attachment for photo]
The target boat is wrapped with 3 x Ta heat shield.
EVAP1 pumped down overnight.
HS water valves were opened this morning, no leaks detected.
IGP1 = 5.5e-7 Torr.
Tapping up TGHT manually to 30A...
Friday, May 01, 2015, 10:54
Tapped up manually to 30A.
Over the course of 20min the vacuum climbed to IGP1 = 1.0 e-5 Torr.
Backed off TGHT to 20A to allow vacuum to stabilize.
Waited ~10min.
Vacuum dropped to IGP1 = 6.5e-6 Torr.
Tapped back-up manually to 30A.
Waited ~45min.
Vacuum stable, IGP1 = 1.2e-5 Torr.
Initiating auto-ramp at 0.1A/min for the TGHT with a max setpoint of 300A / 5.00V.
Good Vacuum = 3.00e-5 Torr. Bad vacuum = 4.00e-5 Torr.
Monday, May 04, 2015, 11:17
IGP1 = 2e-7 Torr.
TGHT = 274A, 4.75V
Ramp-up limited to 275A due to max voltage being set at 5.0V
Increased max voltage to 10V
Tapping up manually to 1800C and recording data.
|
Monday, May 04, 2015, 17:24
Samples have been heated at 1800C for >2 hours.
Vaccum at 4.3e-7 Torr, TGHT 475A/9.1V. (Direct Vol = 5.3V).
Initiated cooling down process. Chamber will be vented tomorrow.
Tuesday, May 05, 2015, 10:22
TGHT reached to 0A. Chamber has already vented.
Samples will be taken out for examination.
|
Friday, May 08, 2015, 15:56, Laura Lambert, , 40282-4, TARGET BOAT, Done, Sintering four different ZrC samples
|
John Wong wrote: |
Laura Lambert wrote: |
Friday, May 01, 2015, 10:27
Four different samples of ZrC are loaded into a target boat.
Sample A: ZrC + NO graphite / hand cut
Sample B: ZrC + NO graphite / laser cut
Sample C: ZrC + graphite / hand cut
Sample D: ZrC + graphite / laser cut
A picture showing the different samples is attached [one face-up/ one face-down sample of each side-by-side]
Each sample consists of ~20-25 discs, stacked together and wrapped in graphite sheet [see attachment for photo]
The target boat is wrapped with 3 x Ta heat shield.
EVAP1 pumped down overnight.
HS water valves were opened this morning, no leaks detected.
IGP1 = 5.5e-7 Torr.
Tapping up TGHT manually to 30A...
Friday, May 01, 2015, 10:54
Tapped up manually to 30A.
Over the course of 20min the vacuum climbed to IGP1 = 1.0 e-5 Torr.
Backed off TGHT to 20A to allow vacuum to stabilize.
Waited ~10min.
Vacuum dropped to IGP1 = 6.5e-6 Torr.
Tapped back-up manually to 30A.
Waited ~45min.
Vacuum stable, IGP1 = 1.2e-5 Torr.
Initiating auto-ramp at 0.1A/min for the TGHT with a max setpoint of 300A / 5.00V.
Good Vacuum = 3.00e-5 Torr. Bad vacuum = 4.00e-5 Torr.
Monday, May 04, 2015, 11:17
IGP1 = 2e-7 Torr.
TGHT = 274A, 4.75V
Ramp-up limited to 275A due to max voltage being set at 5.0V
Increased max voltage to 10V
Tapping up manually to 1800C and recording data.
|
Monday, May 04, 2015, 17:24
Samples have been heated at 1800C for >2 hours.
Vaccum at 4.3e-7 Torr, TGHT 475A/9.1V. (Direct Vol = 5.3V).
Initiated cooling down process. Chamber will be vented tomorrow.
Tuesday, May 05, 2015, 10:22
TGHT reached to 0A. Chamber has already vented.
Samples will be taken out for examination.
|
Friday, May 08, 2015, 15:55
see attachment for data results.
|
Wednesday, May 06, 2015, 13:59, Laura Lambert, , 40282-4, TARGET BOAT, Done, Sintering two different ZrC samples
|
Wednesday, May 06, 2015, 13:54
Two different samples of ZrC are wrapped in graphite sheet and loaded into the target boat.
Sample #1 = ZrC
Sample #2 = ZrC+C
Both samples are hand punched with a 18mm die.
The target boat is wrapped with 3x Ta heat shield.
Pumped down this morning.
HS water valves opened, no leaks detected.
IGP1 = 1.5e-6 Torr.
Tapping up manually to 35A...
Waited ~50min for vacuum to stabilize.
IGP1 = 5.3e-6 Torr.
Initiating auto-ramp at 0.1A/min for the TGHT with a max setpoint of 275A/ 10V
Good vacuum = 3.00e-5 Torr. Bad vacuum = 4.00e-5 Torr.
Wednesday, May 06, 2015, 15:37
Increasing ramping rate to 0.2A/min
Thursday, May 07, 2015, 11:15
Stopping auto ramp.
TGHT = 273A.
Tapping up manually and recording data...
IGP1 = 6.6e-7 Torr.
Thursday, May 07, 2015, 14:21
Increased max voltage to 14V
Friday, May 08, 2015, 09:33
EVAP2 reached 2000C yesterday evening and remained at max setpoint overnight.
IGP1 = 3.8e-7 Torr
Initiated auto-cool this morning at 2.0A/min.
Friday, May 08, 2015, 11:32
IGP1 = 2.1e-7 Torr
TGHT = 221A, 3.21V
OMEGA = 1100C
Increasing auto-cool to 5.0A/min.
Friday, May 08, 2015, 15:53
Vented in air and opened up this afternoon.
See attachment for data results.
|
Friday, April 17, 2015, 16:14, Laura Lambert, SiC, 38817-7, HP-SIS, In progress, Sintering SiC#31
|
Friday, April 17, 2015, 16:01
Total number of foils: 520 discs
Total mass of materials [incl graphite foils]: 60.2441g
Total length packed: 17.0cm
Container is wrapped with 3x Ta-heat shields.
No endcaps inserted to allow outgasing.
Currently being pumped down.
Monday, April 20, 2015, 11:08
Target container is coated with TaC and wrapped with 3-Ta heat shields, not incl center block.
TGHT and TBHT will be ramped up to 820A and 230A, respectively.
Chamber pumped down over the weekend.
IGP1 = 2.1e-7 Torr.
HS cooling water valves opened; no leaks detected.
TGHT max voltage = 18V, TBHT max voltage = 5V
....
attempted to start stepping up manually.
power supply not responding to epics controls for TBHT only...looking into problems now...
Monday, April 20, 2015, 16:06
Epics is working.
Power supply connections unplugged/plugged back in.
Everything working again.
Tapped up manually to 40A.
Waited ~1hr30 for vacuum to stabilize.
IGP1 = 1.8e-6 Torr.
Good vac = 3e-5 Torr. Bad vac = 4e-5 Torr.
TGHT and TBHT will be ramped up to 820A and 230A, respectively.
Initiating auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
Wednesday, April 22, 2015, 15:23
TGHT = 200A, 2.26V; TBHT = 117A, 1.58V
IGP1 = 9.8e-6 Torr.
Increasing auto-ramp to 0.4A/min and 0.2A/min for the TGHT and TBHT respectively.
|
Thursday, April 23, 2015, 10:17, John Wong, SiC, 38817-7, HP-SIS, Done, Sintering SiC#31
|
Laura Lambert wrote: |
Friday, April 17, 2015, 16:01
Total number of foils: 520 discs
Total mass of materials [incl graphite foils]: 60.2441g
Total length packed: 17.0cm
Container is wrapped with 3x Ta-heat shields.
No endcaps inserted to allow outgasing.
Currently being pumped down.
Monday, April 20, 2015, 11:08
Target container is coated with TaC and wrapped with 3-Ta heat shields, not incl center block.
TGHT and TBHT will be ramped up to 820A and 230A, respectively.
Chamber pumped down over the weekend.
IGP1 = 2.1e-7 Torr.
HS cooling water valves opened; no leaks detected.
TGHT max voltage = 18V, TBHT max voltage = 5V
....
attempted to start stepping up manually.
power supply not responding to epics controls for TBHT only...looking into problems now...
Monday, April 20, 2015, 16:06
Epics is working.
Power supply connections unplugged/plugged back in.
Everything working again.
Tapped up manually to 40A.
Waited ~1hr30 for vacuum to stabilize.
IGP1 = 1.8e-6 Torr.
Good vac = 3e-5 Torr. Bad vac = 4e-5 Torr.
TGHT and TBHT will be ramped up to 820A and 230A, respectively.
Initiating auto-ramp at 0.2A/min and 0.1A/min for the TGHT and TBHT respectively.
Wednesday, April 22, 2015, 15:23
TGHT = 200A, 2.26V; TBHT = 117A, 1.58V
IGP1 = 9.8e-6 Torr.
Increasing auto-ramp to 0.4A/min and 0.2A/min for the TGHT and TBHT respectively.
|
Thursday, April 23, 2015, 10:15
Vac at 2.e-6 Torr. Increased TGHT ramping rate to 1.0A/min. Current temperature at 1443C, TGHT at 641A, TBHT at 230A.
Thursday, April 23, 2015, 15:02
Evap#2 window for the temp reader is now coated, so temp reading is not available. (see attachment).
TGHT has been at 820A/13.45V for almost 2 hours, will continue to heat at this current for a few more hours. Will initiate the cooling process from home…
Thursday, April 23, 2015, 22:31
Target has been heated at 820A for about 9.5hrs. Current vacuum at 4.7e-7 Torr.
Initiating cooling process at -2A/min for TGHT and -1A/min for TBHT.
Friday, April 24, 2015, 10:13
Target has been cooled at 0A for about 5 hours. Chamber is currently being vented and the target will be taken out for inspection.
Friday, April 24, 2015, 12:37
The target was inspected.
Some yellow crystals were form around the ends but they were easily removed this time.
With both ends open during the sintering process and shorten the target length with 1cm space of both side, the target is looking a lot better.
No visible damage on the target surface.
Inside, the channel has a clear pathway, and the discs are nicely aligned.
End caps and Rh foils are inserted - It's ready for assembly.
See link for pics after the sintering process.
https://www.dropbox.com/sh/w5k4l3fezfat2cm/AAAyX67zyUPUVvN_WzEHFXM2a?dl=0
|
Thursday, April 09, 2015, 09:38, Laura Lambert, Empty, 38817-7, HP-SIS, Done, Sintering TaC coating container for SiC#32
|
Thursday, April 09, 2015, 09:33
Target container is coated with TaC and wrapped with 3-Ta heat shields, not incl center block.
TGHT and TBHT will be ramped up to 820A and 230A, respectively.
Chamber pumped down overnight.
IGP1 = 5.2e-7 Torr.
HS cooling water valves opened; no leaks detected.
TGHT max voltage = 18V, TBHT max voltage = 5V
Stepping TGHT and TBHT up to 35A...
Thursday, April 09, 2015, 10:07
Waited ~20min, vacuum stable.
IGP1 = 5.3e-7 Torr.
Good vac = 3e-5 Torr. Bad vac = 4e-5 Torr.
Auto-ramp initiated at 0.2A/min.
Monday, April 13, 2015, 09:06
Reached max setpoints sunday morning [see attached photo for striptool].
Internal temperature measured with OMEGA = 1965C
IGP1 = 4.4e-7 Torr,
Initiating auto cool for TGHT and TBHT at 2.0A/min and 1.0A/min respectively.
Tuesday, April 14, 2015, 14:12
Vented in air and opened up this morning.
Fully sintered.
|
Monday, March 09, 2015, 16:50, Laura Lambert, Ta, 38817-5, HP-SIS, In progress, Conditioning Ta target
|
Monday, March 09, 2015, 16:47
Target consists of 400 discs.
Total packed length 3.4cm
Total mass 45.8181g
Re foil inserted.
Chamber is currently being pumped down.
No Ta-heat shield wrapped.
One end-cap inserted on left (wrt ionizer into the page)
TGHT and TBHT will be ramped up to 820A/230A respectively at 2.0A/min.
Tuesday, March 10, 2015, 10:28
HS water valves opened, no leaks detected.
IGP1 = 4.5e-7 Torr.
Power supply not responding to epics...AGAIN. grrrr
Tuesday, March 10, 2015, 13:17
IOC was rebooted - back up and running again! yay!
IGP1 = 4.0e-7 Torr.
Tapped up manually to 35A, waited ~30min, vaccuum stable.
Initiating auto-ramp.
Vacuum limit stop at 5.0e-5 Torr, backing off at 6.0e-5 Torr.
Wednesday, March 11, 2015, 09:11
Target has been at max setpoints for ~14hrs.
OMEGA = 1472C
TGHT = 820A, 12.85V
TBHT = 230A, 3.696V
IGP1 = 5.5ee-7 Torr
Manually tapping up to obtain hotter internal temperature...
Wednesday, March 11, 2015, 11:33
Current conditions:
OMEGA = 1565C
TGHT = 900A, 14.3V
TBHT = 230A, 3.7V
IGP1 = 6.3e-7 Torr
Digital pyrometer readings:
Hottest point on left leg, WRT ionizer tube into page = 2400C
Internal temp of container = 1580C
Sat at this temperature ~45min.
Initiating auto-cool at TGHT 2.0A/min, TBHT 1.0A/min
[See attached photo for collected data]
Thursday, March 12, 2015, 13:12
vented and opened up this morning.
only reached a max internal temp of 1580C.
therefore added 3xTa heat shield and will re-condition at a higher temp.
currently pumping back down.
Thursday, March 12, 2015, 14:34
IGP1 = 7.0e-7 Torr
stepped up to 35A, waited ~30min, vacuum stable.
IGP1 = 6.1e-7 Torr
Initating ramp-up...
Friday, March 13, 2015, 07:47
IGP1 = 2.9e-7 Torr
reached max set points for TGHT = 600A, TBHT = 230A
Initiating manual tap-up.
Friday, March 13, 2015, 10:31
Reached 720A, 1800C at 0850
Will continue to heat for ~3hrs
[see attachment for collected data]
Friday, March 13, 2015, 12:00
Sat at max temperature, 1800C, for 3 hours.
Initiating auto-cool at 2.0A/min for TGHT and 1.0A/min for TBHT.
|
Monday, March 16, 2015, 17:38, John Wong, Ta, 38817-5, HP-SIS, Done, Conditioning Ta target
|
Laura Lambert wrote: |
Monday, March 09, 2015, 16:47
Target consists of 400 discs.
Total packed length 3.4cm
Total mass 45.8181g
Re foil inserted.
Chamber is currently being pumped down.
No Ta-heat shield wrapped.
One end-cap inserted on left (wrt ionizer into the page)
TGHT and TBHT will be ramped up to 820A/230A respectively at 2.0A/min.
Tuesday, March 10, 2015, 10:28
HS water valves opened, no leaks detected.
IGP1 = 4.5e-7 Torr.
Power supply not responding to epics...AGAIN. grrrr
Tuesday, March 10, 2015, 13:17
IOC was rebooted - back up and running again! yay!
IGP1 = 4.0e-7 Torr.
Tapped up manually to 35A, waited ~30min, vaccuum stable.
Initiating auto-ramp.
Vacuum limit stop at 5.0e-5 Torr, backing off at 6.0e-5 Torr.
Wednesday, March 11, 2015, 09:11
Target has been at max setpoints for ~14hrs.
OMEGA = 1472C
TGHT = 820A, 12.85V
TBHT = 230A, 3.696V
IGP1 = 5.5ee-7 Torr
Manually tapping up to obtain hotter internal temperature...
Wednesday, March 11, 2015, 11:33
Current conditions:
OMEGA = 1565C
TGHT = 900A, 14.3V
TBHT = 230A, 3.7V
IGP1 = 6.3e-7 Torr
Digital pyrometer readings:
Hottest point on left leg, WRT ionizer tube into page = 2400C
Internal temp of container = 1580C
Sat at this temperature ~45min.
Initiating auto-cool at TGHT 2.0A/min, TBHT 1.0A/min
[See attached photo for collected data]
Thursday, March 12, 2015, 13:12
vented and opened up this morning.
only reached a max internal temp of 1580C.
therefore added 3xTa heat shield and will re-condition at a higher temp.
currently pumping back down.
Thursday, March 12, 2015, 14:34
IGP1 = 7.0e-7 Torr
stepped up to 35A, waited ~30min, vacuum stable.
IGP1 = 6.1e-7 Torr
Initating ramp-up...
Friday, March 13, 2015, 07:47
IGP1 = 2.9e-7 Torr
reached max set points for TGHT = 600A, TBHT = 230A
Initiating manual tap-up.
Friday, March 13, 2015, 10:31
Reached 720A, 1800C at 0850
Will continue to heat for ~3hrs
[see attachment for collected data]
Friday, March 13, 2015, 12:00
Sat at max temperature, 1800C, for 3 hours.
Initiating auto-cool at 2.0A/min for TGHT and 1.0A/min for TBHT.
|
Monday, March 16, 2015, 17:30
Target was removed from Evap#2. It was successfully conditioned.
The other end cap was inserted and expended.
Standard salts were added. And Re foil is inserted.
Target is ready for assembly.
|
Thursday, February 19, 2015, 15:21, Laura Lambert, Empty, 41177-2, LP-SIS, Done, Sintering TaC coating container for UCx#12
|
Thursday, February 19, 2015, 15:19
Target container coated with TaC, loaded in EVAP2.
No Ta heat shields.
Will pump down over the weekend.
Monday, February 23, 2015, 10:22
IGP1 = 1.75e-7 Torr
TGHT will be ramped up to 580A at 0.2A/min
TBHT will be ramped up to 230A at 0.2A/min
evap2 power supply not responding to epics controls...waiting on fix
Wednesday, February 25, 2015, 16:05
controls now fixed.
danceioc1 involving evap ioc will be updated tomorrow by controls.
once ioc update complete will ramp up.
Friday, February 27, 2015, 09:34
ioc update complete yesterday afternoon.
IGP1 = 1.1e-7
initiating ramp up...
Parameter setup: 5.0e-5 good vac, 6.0e-5 bad vac.
Monday, March 02, 2015, 09:01
IGP1 = 2.5e-7 Torr
TGHT = 578A
TBHT = 232A
OMEGA = 1750C
Increasing to 1800C
Monday, March 02, 2015, 10:42
Reached 1800C at 10:30
TGHT = 603A
TBHT = 232A
IGP1 = 2.8e-7 Torr
Monday, March 02, 2015, 14:26
Sat at max set point for 4hrs.
IGP1 = 2.7e-7 Torr.
Initiating auto-cool, TGHT @ 2A/min, TBHT @ 1A/min.
Tuesday, March 03, 2015, 09:17
vented and opened this a.m.
target container looks good, TaC coating fully sintered.
|
Wednesday, February 11, 2015, 16:12, Laura Lambert, Empty, 41077-2, LP-SIS, Done, Conditioning graphite insert inside container - with heat shield
|
Wednesday, February 11, 2015, 16:10
Container loaded into EVAP2.
3xTa heat shields.
Chamber currently being pumped down.
TGHT/ TBHT will be ramped up to 580A/ 230A or 1800C tapped up manually.
Thursday, February 12, 2015, 09:39
HS water valves opened, no leaks detected.
Tapping up manually.
Thursday, February 12, 2015, 12:07
OMEGA reached 1805C; TGHT = 415A, TBHT = 205A
Will continue to tap up manually to 2000C
Thursday, February 12, 2015, 15:19
Reached TGHT = 500A, TBHT = 230A, OMEGA = 2035C.
Sat for ~2hrs.
Tapping up a further 25A on the TGHT.
Thursday, February 12, 2015, 16:05
Tapped up manually to:
OMEGA = 2250C
DV = 5.65V
TGHT = 580A
TBHT = 230A
Friday, February 13, 2015, 10:05
Reached max setpoint last night.
Voltage starting to increase at contant TGHT @ 580A. Lower TGHT to 525A, temp at 2150C (time 6:30pm)
Initiating manual cool down.
Friday, February 13, 2015, 15:31
vented and opened up this afternoon.
everything looked good, container not broken! graphite insert looked good! the container was slightly bent, but nothing of significance.
however, the graphite insert bonded to the container so it was not taken out in one piece... |
Tuesday, February 10, 2015, 14:01, Laura Lambert, Empty, 41077-2, LP-SIS, Done, Conditioning graphite insert inside container - no heat shield
|
Tuesday, February 10, 2015, 14:00
Container loaded into EVAP2 at noon.
no heat shields.
Chamber currently being pumped down.
TGHT/ TBHT will be ramped up to 580A/ 230A, tapped up manually.
Tuesday, February 10, 2015, 14:39
HS water valves opened, no leaks detected.
Tapping up manually / recording data in excel
Wednesday, February 11, 2015, 11:24
Reached max set points yesterday early evening.
Tapped down manually this a.m.
Will vent and open this afternoon.
Wednesday, February 11, 2015, 15:54
Took out this afternoon.
container looks good.
graphite insert removed/ inspected - not much change, slightly lighter in colour.
[see attachments for graphs/ table]
|
Monday, February 02, 2015, 16:33, John Wong, Empty, 41077-2, LP-SIS, In progress, Coating/Sintering TaC on target container - For Graphite Insert
|
Monday, February 02, 2015, 16:28
Container is coated with TaC. No Ta foil wrapped around.
Chamber is being pumped down.
TGHT/TBHT will be ramped up to 580A/230A at 0.2A/min.
|
Tuesday, February 03, 2015, 10:31, Laura Lambert, Empty, 41077-2, LP-SIS, In progress, Coating/Sintering TaC on target container - For Graphite Insert
|
John Wong wrote: |
Monday, February 02, 2015, 16:28
Container is coated with TaC. No Ta foil wrapped around.
Chamber is being pumped down.
TGHT/TBHT will be ramped up to 580A/230A at 0.2A/min.
|
Tuesday, February 03, 2015, 10:28
HS water valves opened; no leaks detected.
IGP1 = 5.9e-7 Torr
Wednesday, February 04, 2015, 11:10
attempted to initiate manual ramp up of TGHT and TBHT yesterday, but not responding to EPICS
currently sitting under vacuum, waiting on fix...
Wednesday, February 04, 2015, 14:16
controls fixed.
initiated auto-ramp.
Thursday, February 05, 2015, 08:56
IGP1 = 4.1e-7 Torr
TGHT = 290A
TBHT = 225A
Increasing auto-ramp to 1.0A/min
Thursday, February 05, 2015, 13:49
IGP1 = 1.4e-6 Torr
TGHT = 569A
TBHT = 232A
Increasing auto-ramp to 2.0A/min
|
Thursday, February 05, 2015, 18:03, John Wong, Empty, 41077-2, LP-SIS, In progress, Coating/Sintering TaC on target container - For Graphite Insert
|
Laura Lambert wrote: |
John Wong wrote: |
Monday, February 02, 2015, 16:28
Container is coated with TaC. No Ta foil wrapped around.
Chamber is being pumped down.
TGHT/TBHT will be ramped up to 580A/230A at 0.2A/min.
|
Tuesday, February 03, 2015, 10:28
HS water valves opened; no leaks detected.
IGP1 = 5.9e-7 Torr
Wednesday, February 04, 2015, 11:10
attempted to initiate manual ramp up of TGHT and TBHT yesterday, but not responding to EPICS
currently sitting under vacuum, waiting on fix...
Wednesday, February 04, 2015, 14:16
controls fixed.
initiated auto-ramp.
Thursday, February 05, 2015, 08:56
IGP1 = 4.1e-7 Torr
TGHT = 290A
TBHT = 225A
Increasing auto-ramp to 1.0A/min
Thursday, February 05, 2015, 13:49
IGP1 = 1.4e-6 Torr
TGHT = 569A
TBHT = 232A
Increasing auto-ramp to 2.0A/min
|
Thursday, February 05, 2015, 18:02
Auto-cooling TGHT to 400A at 1A/min. Need to take voltage reading tomorrow.
|
Tuesday, February 10, 2015, 13:19, Laura Lambert, Empty, 41077-2, LP-SIS, Done, Coating/Sintering TaC on target container - For Graphite Insert
|
John Wong wrote: |
Laura Lambert wrote: |
John Wong wrote: |
Monday, February 02, 2015, 16:28
Container is coated with TaC. No Ta foil wrapped around.
Chamber is being pumped down.
TGHT/TBHT will be ramped up to 580A/230A at 0.2A/min.
|
Tuesday, February 03, 2015, 10:28
HS water valves opened; no leaks detected.
IGP1 = 5.9e-7 Torr
Wednesday, February 04, 2015, 11:10
attempted to initiate manual ramp up of TGHT and TBHT yesterday, but not responding to EPICS
currently sitting under vacuum, waiting on fix...
Wednesday, February 04, 2015, 14:16
controls fixed.
initiated auto-ramp.
Thursday, February 05, 2015, 08:56
IGP1 = 4.1e-7 Torr
TGHT = 290A
TBHT = 225A
Increasing auto-ramp to 1.0A/min
Thursday, February 05, 2015, 13:49
IGP1 = 1.4e-6 Torr
TGHT = 569A
TBHT = 232A
Increasing auto-ramp to 2.0A/min
|
Thursday, February 05, 2015, 18:02
Auto-cooling TGHT to 400A at 1A/min. Need to take voltage reading tomorrow.
|
Tuesday, February 10, 2015, 09:35
Vented and opened this morning.
Container fully sintered.
|
Thursday, January 22, 2015, 14:21, Anders Mjos, Empty, , , Problems resolved, CG1A replaced
|
See previous e-log entry for details |
Wednesday, January 14, 2015, 13:46, Anders Mjos, Empty, , , Maintenance, Pumping down for water leak test
|
Wednesday, January 14, 2015, 13:46: Roughing
Wednesday, January 14, 2015, 14:57: Starting turbo
Monday, January 19, 2015, 13
Water opened up to one circuit at at time. No response on the vacuum could be seen.
IGP1 at 1.7E-7 T
IGP2 at 3E-8 T
Tuesday, January 20, 2015, 13:11: Stopped turbo and roughing pump.
Wednesday, January 21, 2015, 15:46: Venting
Rick and Anders found CG1A to be reading too high a value. A borrowed gauge from the vacuum group confirmed this. A new gauge will be installed
Thursday, January 22, 2015, 14:06: Roughing
Thursday, January 22, 2015, 14:18: Venting
The reading is consistent between CG1A and CG1B, which simplifies pump down. |
Thursday, December 11, 2014, 10:20, Laura Lambert, , , , Maintenance, water supply shut off for lab closure over holidays
|
Thursday, December 11, 2014, 10:17
water supply and return valves closed for lab closure over the holidays.
all taps leading into evap2 have been closed.
evap2 was fully flushed leaving no water left inside the system.
|
Wednesday, November 26, 2014, 14:09, Laura Lambert, , , , Maintenance, OMEGA-IR dark patch and backing pump trip
|
Wednesday, November 26, 2014, 13:47
OMEGA-IR laser had a dark patch on it [see picture]
Cleaned window, still dark patch
When tested by itself, through air, not through window, patch still visible - cleaned lens of OMEGA-IR, still no change.
Conclusion: assuming laser used to be able to focus the OMEGA-IR to a specific area - so visual only, but the measurements itself will not be affected.
Wednesday, November 26, 2014, 13:53
Backing pump trips off every time roughing valve turned on through epics.
Requested further investigation...
Friday, November 28, 2014, 12:09
Backing Pump has been replaced, waiting on a reply from OMEGA re: dark patch on laser
Pancake monitor was also acting funny. Background was reading 100cpm and jumping up to as high as 400cpm by simply moving the probe piece.
The wire connecting the probe to the monitor was replaced and works fine now.
Tuesday, December 09, 2014, 15:55
Finally got a reply from the OMEGA people:
"That [ dark patch] would happen because of sharp bends in the fiber, or simply defective fiber cable.
As manufacturer we allow 2% of broken fibers, out of 870 in the bundle.
As far as measurements is concerned, if IR2 is used in dual colour mode,
the field of view can be obstructed as much as 50%,
without changing the readings accuracy. This laser issure should not affect readings."
-Quote from Brian Newport from OMEGA
|
Wednesday, November 19, 2014, 15:10, Laura Lambert, Empty, 39530-2, LP-FEBIAD, Done, test#1. direct voltage and OMEGA temperature measurements
|
Wednesday, November 19, 2014, 15:10
currently pumping down
Wednesday, November 19, 2014, 15:28
container is wrapped with 3 x Ta-heat shield
leak check done
Starting voltage = -0.017mV
TGHT = 0A, 0V
TBHT = 0A, 0V
IGP1 = 1.7e-6 Torr
Wednesday, November 19, 2014, 16:33
Tapped TGHT up manually to 100A
DV [direct voltage] = 0.33V
TGHT = 109A
TBHT = 0A
IGP1 = 1.3e-6 Torr
Initiating auto-ramp of TGHT to 400A at 2A/min
Thursday, November 20, 2014, 09:49
DV = 3.47V
OMEGA = 1645C
TGHT = 401A, 6.49V
TBHT = 0
IGP1 = 4.5e-7Torr
TGHT finished auto-ramping ~19:00 last night
initiating manual tap up to 2000 celsius or 580A [whichever is higher] and recording activity
Friday, November 21, 2014, 12:50
TGHT was ramped up to 580A yesterday and left overnight.
In the picture attached one can see the TGHT current has remained constant at 578A [red = TGHT current, green = TGHT voltage]
The vacuum has slowly gone down as expected.
However, the DV, TGHT voltage and temperature have deviated. They have dipped up and down several times throughout the night. The first deviation was observed ~3.5hours after it reached its target of 580A.
DV reached 6.02V [when TGHT initially hit 580A] and increased to 6.27V after 3.5hrs and is currently sitting at 5.94V
OMEGA reached 2111C [when TGHT initially hit 580A] and increased to 2154C after 3.5 hrs and is currently sitting at 2094C
TGHT voltage reached 10.4V [when TGHT initially hit 580A] and increased to 10.6V after 3.5hrs and is currently sitting at 10.3V
Friday, November 21, 2014, 17:59
EVAP2 sat at max setting: TGHT = 580A and TBHT = 230A for ~4hours
Initiating auto-cool TGHT 2A/min, TBHT 1A/min
Monday, November 24, 2014, 14:28
Vented and opened this morning.
No notable changes on target container.
[See attachments for more detailed information of results]
|
Monday, November 10, 2014, 13:55, Laura Lambert, Empty, , LP-SIS, Done, Sintering TaC coating container for UCx#11 [2nd container]
|
Monday, November 10, 2014, 13:51
target container was sprayed with TaC on friday and sintered over the weekend.
vented and removed from evap2 this morning, looks good.
this container will be used as a round2 for UCx #11 since the last container broke as it was being assembled.
hopefully all the materials can be recovered and re-used/re-loaded into the new container...
|
Thursday, October 23, 2014, 15:38, Laura Lambert, SiC, 39530-8, HP-FEBIAD, In progress, Testing the new OMEGA-IR2C on SiC#31 target
|
Thursday, October 23, 2014, 15:34
*See elog #142 for target description*
one endcap still in place, one removed for OMEGA-IR2C beam to reach material [see pic]
no heat shields
currently being pumped down
Friday, October 24, 2014, 11:34
EVAP2 pumped down overnight.
IGP1 = 7e-7 Torr
HS water valves opened, no leaks detected.
TGHT will be ramped up to 1400C
TBHT will be ramped up to 230A
Friday, October 24, 2014, 14:32
TBHT reached 230A, TGHT reached 1400C
Stepped TGHT up manually to 1600C; TGHT = 693A, 10.6V [see pic]
Friday, October 24, 2014, 15:58
TGHT = 760A, 12.07V [local read back] = setpoint.
epics readback TGHT = 754.8A, 11.76V
OMEGA = 1700C
Friday, October 24, 2014, 16:26
OMEGA = 1800C
epics readback TGHT = 828.7A, 13.15V
Friday, October 24, 2014, 16:34
OMEGA = 1900C
epics readback TGHT = 899A, 14.53V
Friday, October 24, 2014, 16:46
OMEGA = 2000C
epics readback TGHT = 967A, 15.8V
MIKRON target spot on SiC = 1650C, e = 0.97
|
Tuesday, November 04, 2014, 16:21, John Wong, SiC, 39530-8, HP-FEBIAD, Done, Testing the new OMEGA-IR2C on SiC#31 target (NOT TO BE USED ONLINE)
|
Laura Lambert wrote: |
Thursday, October 23, 2014, 15:34
*See elog #142 for target description*
one endcap still in place, one removed for OMEGA-IR2C beam to reach material [see pic]
no heat shields
currently being pumped down
Friday, October 24, 2014, 11:34
EVAP2 pumped down overnight.
IGP1 = 7e-7 Torr
HS water valves opened, no leaks detected.
TGHT will be ramped up to 1400C
TBHT will be ramped up to 230A
Friday, October 24, 2014, 14:32
TBHT reached 230A, TGHT reached 1400C
Stepped TGHT up manually to 1600C; TGHT = 693A, 10.6V [see pic]
Friday, October 24, 2014, 15:58
TGHT = 760A, 12.07V [local read back] = setpoint.
epics readback TGHT = 754.8A, 11.76V
OMEGA = 1700C
Friday, October 24, 2014, 16:26
OMEGA = 1800C
epics readback TGHT = 828.7A, 13.15V
Friday, October 24, 2014, 16:34
OMEGA = 1900C
epics readback TGHT = 899A, 14.53V
Friday, October 24, 2014, 16:46
OMEGA = 2000C
epics readback TGHT = 967A, 15.8V
MIKRON target spot on SiC = 1650C, e = 0.97
|
Tuesday, November 04, 2014, 15:59
Target was heated up to 2000C and last for about 1.5 days before the right leg (ionizer points into the page) broke off.
Interesting discovery... The "yellowish" crystals are forming on the discs.
Suspecting a phase transformation of 6H (hexagonal/- alpha SiC (hexagonal) polytype to 3C(cubic) - beta SiC
More study needs to be done...
See elog # 168.
The leg of this target was repaired in the Machine shop.
THIS TARGET WILL NOT BE USED ONLINE - IT WILL BE USED FOR OFFLINE R&D PURPOSES.
|
Tuesday, November 04, 2014, 16:20, John Wong, SiC, , TARGET BOAT, In progress, TEST: Fabrication of SiC & Determine phase transformation 3C vs 6H
|
Tuesday, November 04, 2014, 16:08
The purpose of this experiment is to improve the fabrication of SiC. Previously, the SiC target was heated to 2000c and yellow crystals were observed.
In this experiment, 10g of SiC powder (7um size) was previously milled down (actual size to be determined under SEM). The powder was mixed with 5% PVA and the slurry was pour onto a glass and let dry. The semi-dry slurry was rolled up into balls. The SiC balls were let dry in over (115C) over night. Taken out 2.903g SiC + 5% PVA, it's rolled up with a small sheet of graphite foil. Then the targer boat is filled with the sample and wrapped with 3-layers of Ta-heat shield.
The sample will be heated up to 2000C to see if the yellow crystals are reproducible. It is suspected that there might be a phase transformation from 6H alpha-SiC to 3C beta-SiC.
Chamber is currently being pumped down...
Wednesday, November 05, 2014, 14:04
TGHT was ramped up over night, currently at 485A = 1800 C.
Will do manual step up to get to 2000C.
|
Thursday, October 09, 2014, 17:41, John Wong, Nb, , TARGET BOAT, Done, Conditioning Nb targets (for Bob)
|
Thursday, October 09, 2014, 17:36
Target boat consists of 5 Nb discs. Each disc is wrapped with Nb foil, and to be heated to 1400C for 4 hours.
Chamber has been pumped down to 6.5e-7 Torr. HS valves open - no leaks detected.
TGHT has ramped to 330A to maintain the 1400C temperature.
At 21:30, the target will be cooled down.
Temperature can be monitored from this link:
https://www.dropbox.com/sh/kor6gnutnlimqxw/AAAee2yb-Hj3JEbBysrAW2oYa?dl=0
Thursday, October 09, 2014, 22:48
Samples have been heated at 1420C for over 4 hours.
Pressure at 6.6 e-7 Torr.
Cooling process initiated, ramping down at 2A/min.
Friday, October 10, 2014, 13:50
Samples were successfully conditions; no signs of any damage.
|
Thursday, October 02, 2014, 11:52, Laura Lambert, Empty, 40282-5, LP-SIS, In progress, Sintering TaC coating container for UCx#11
|
Thursday, October 02, 2014, 11:51
Target container sprayed with TaC, currently drying in fume hood
Monday, October 06, 2014, 12:11
Target container & back block is wrapped with 3 layers of Ta-heat shield. The chamber has been pumped down over the weekend.
Pressure currently at 2.23e-7 Torr.
HS water valves open; no leaks detected.
TGHT will be ramped up to 580A at 0.2A/min
TBHT will be ramped up to 230A at 0.2A/min.
|
Monday, October 06, 2014, 12:17, John Wong, Empty, 40282-5, LP-SIS, In progress, Sintering TaC coating container for UCx#11 (temp measured with OMEGA 2IR)
|
Laura Lambert wrote: |
Thursday, October 02, 2014, 11:51
Target container sprayed with TaC, currently drying in fume hood
Monday, October 06, 2014, 12:11
Target container & back block is wrapped with 3 layers of Ta-heat shield. The chamber has been pumped down over the weekend.
Pressure currently at 2.23e-7 Torr.
HS water valves open; no leaks detected.
TGHT will be ramped up to 580A at 0.2A/min
TBHT will be ramped up to 230A at 0.2A/min.
|
Monday, October 06, 2014, 12:16
Stepped up both TGHT/TBHT to 35A.
Tuesday, October 07, 2014, 12:54
TBHT reached to 230A/3.7V and TGHT is still ramping up, currently at 303A/4.5V. Temp measured with Omega-IR2 = 1165C with e'=0.85
Pressure @ 5.2e-7 Torr.
Increase ramping rate to 2A/min.
Tuesday, October 07, 2014, 16:21
TGHT is now at 580A and TGHT at 230A.
Temperature is measured with OMEGA-IR2, MIKRON, and analog pyrometer - All the measurements are agreed at 1700C (without the tantalum emissivity correction of 250C)
The OMEGA-IR2 slope has changed to 0.97 for the correction - The real temperature reading from the display is showing 1935C.
Now... attempting to low TBHT to see any temperature change.
Tuesday, October 07, 2014, 17:01
TGHT @ 580A.
TBHT = 180C, Temp = 1925C
TBHT = 130C, Temp = 1920C
Not much of change in the temperature on the target tube...
Tuesday, October 07, 2014, 17:07
Attempting to increase the temperature to 2000C
TGHT = 600A, Temp = 1955C
TGHT = 620A, Temp = 2000C
Target will continue heating at this temperature overnight... Will continue to monitor.
Tuesday, October 07, 2014, 20:59
After almost 4 hours of heating at 620A on TGHT, the temperature has dropped to 1980C.
Pressure is coming down to 1.17e-6 Torr.
Increased TGHT to 630A to maintain temp @ 2000C
|
Wednesday, October 08, 2014, 11:51, Laura Lambert, Empty, 40282-5, LP-SIS, Done, Sintering TaC coating container for UCx#11 (temp measured with OMEGA 2IR)
|
John Wong wrote: |
Laura Lambert wrote: |
Thursday, October 02, 2014, 11:51
Target container sprayed with TaC, currently drying in fume hood
Monday, October 06, 2014, 12:11
Target container & back block is wrapped with 3 layers of Ta-heat shield. The chamber has been pumped down over the weekend.
Pressure currently at 2.23e-7 Torr.
HS water valves open; no leaks detected.
TGHT will be ramped up to 580A at 0.2A/min
TBHT will be ramped up to 230A at 0.2A/min.
|
Monday, October 06, 2014, 12:16
Stepped up both TGHT/TBHT to 35A.
Tuesday, October 07, 2014, 12:54
TBHT reached to 230A/3.7V and TGHT is still ramping up, currently at 303A/4.5V. Temp measured with Omega-IR2 = 1165C with e'=0.85
Pressure @ 5.2e-7 Torr.
Increase ramping rate to 2A/min.
Tuesday, October 07, 2014, 16:21
TGHT is now at 580A and TGHT at 230A.
Temperature is measured with OMEGA-IR2, MIKRON, and analog pyrometer - All the measurements are agreed at 1700C (without the tantalum emissivity correction of 250C)
The OMEGA-IR2 slope has changed to 0.97 for the correction - The real temperature reading from the display is showing 1935C.
Now... attempting to low TBHT to see any temperature change.
Tuesday, October 07, 2014, 17:01
TGHT @ 580A.
TBHT = 180C, Temp = 1925C
TBHT = 130C, Temp = 1920C
Not much of change in the temperature on the target tube...
Tuesday, October 07, 2014, 17:07
Attempting to increase the temperature to 2000C
TGHT = 600A, Temp = 1955C
TGHT = 620A, Temp = 2000C
Target will continue heating at this temperature overnight... Will continue to monitor.
Tuesday, October 07, 2014, 20:59
After almost 4 hours of heating at 620A on TGHT, the temperature has dropped to 1980C.
Pressure is coming down to 1.17e-6 Torr.
Increased TGHT to 630A to maintain temp @ 2000C
|
Wednesday, October 08, 2014, 11:46
Temperature readout from omega-IR2C = 2054C
TGHT = 11.14V, 628.0A
TBHT = 2.01V, 129.8A
IGP1 = 8.2e-7Torr
Initiating auto-cool for TGHT @ 2A/min, TBHT @ 1A/min
Thursday, October 09, 2014, 16:00
vented in air and opened up this morning
target container looks good!
|
Thursday, October 09, 2014, 16:37, John Wong, Empty, 40282-5, LP-SIS, Done, Sintering TaC coating container for UCx#11 (temp measured with OMEGA 2IR)
|
Laura Lambert wrote: |
John Wong wrote: |
Laura Lambert wrote: |
Thursday, October 02, 2014, 11:51
Target container sprayed with TaC, currently drying in fume hood
Monday, October 06, 2014, 12:11
Target container & back block is wrapped with 3 layers of Ta-heat shield. The chamber has been pumped down over the weekend.
Pressure currently at 2.23e-7 Torr.
HS water valves open; no leaks detected.
TGHT will be ramped up to 580A at 0.2A/min
TBHT will be ramped up to 230A at 0.2A/min.
|
Monday, October 06, 2014, 12:16
Stepped up both TGHT/TBHT to 35A.
Tuesday, October 07, 2014, 12:54
TBHT reached to 230A/3.7V and TGHT is still ramping up, currently at 303A/4.5V. Temp measured with Omega-IR2 = 1165C with e'=0.85
Pressure @ 5.2e-7 Torr.
Increase ramping rate to 2A/min.
Tuesday, October 07, 2014, 16:21
TGHT is now at 580A and TGHT at 230A.
Temperature is measured with OMEGA-IR2, MIKRON, and analog pyrometer - All the measurements are agreed at 1700C (without the tantalum emissivity correction of 250C)
The OMEGA-IR2 slope has changed to 0.97 for the correction - The real temperature reading from the display is showing 1935C.
Now... attempting to low TBHT to see any temperature change.
Tuesday, October 07, 2014, 17:01
TGHT @ 580A.
TBHT = 180C, Temp = 1925C
TBHT = 130C, Temp = 1920C
Not much of change in the temperature on the target tube...
Tuesday, October 07, 2014, 17:07
Attempting to increase the temperature to 2000C
TGHT = 600A, Temp = 1955C
TGHT = 620A, Temp = 2000C
Target will continue heating at this temperature overnight... Will continue to monitor.
Tuesday, October 07, 2014, 20:59
After almost 4 hours of heating at 620A on TGHT, the temperature has dropped to 1980C.
Pressure is coming down to 1.17e-6 Torr.
Increased TGHT to 630A to maintain temp @ 2000C
|
Wednesday, October 08, 2014, 11:46
Temperature readout from omega-IR2C = 2054C
TGHT = 11.14V, 628.0A
TBHT = 2.01V, 129.8A
IGP1 = 8.2e-7Torr
Initiating auto-cool for TGHT @ 2A/min, TBHT @ 1A/min
Thursday, October 09, 2014, 16:00
vented in air and opened up this morning
target container looks good!
|
Thursday, October 09, 2014, 16:36
Photos for the OMEGA-IR2C temp measurement can be found on this link (see also the subfolder for the heating process):
https://www.dropbox.com/sh/n5sxcepg7e847xw/AACMubuKW1idd49D1Nz_0diNa?dl=0 |
Thursday, October 09, 2014, 15:59, John Wong, Nb, , TARGET BOAT, In progress, Conditioning Nb target (for Bob)
|
Thursday, October 09, 2014, 15:56
The target boat contains 5 samples of Nb discs. Each disc is wrapped with Nb foil and labelled.
Samples will be heated up to 1400C for 4 hours.
chamber has been pumped down to 3.9e-6 Torr. HS valves open - no leaks detected.
Ramping up TGHT...
|
Thursday, October 02, 2014, 11:26, John Wong, Empty, , , Maintenance, Broken insulators
|
Thursday, October 02, 2014, 11:22
It was found that after the last process, Evap#2 has broken insulators - the cylinder insulator that supports the target centre legs and the block insulator that supports the terminals.
Informed Anders/Rick.
|
Friday, October 03, 2014, 13:02, Anders Mjos, Empty, , , Maintenance, Broken insulators
|
John Wong wrote: |
Thursday, October 02, 2014, 11:22
It was found that after the last process, Evap#2 has broken insulators - the cylinder insulator that supports the target centre legs and the block insulator that supports the terminals.
Informed Anders/Rick.
|
Friday, October 03, 2014
- Insulators replaced. Torque 55 in lbs on all fasteners.
- Cleaned TGHT terminals with scotch-brite and methanol.
- New (clean) heat shield prepared WO-39230-2.
- Re-installed right side heat shield alignment pin (previously removed to allow line of sight to the target).
|
Thursday, September 25, 2014, 17:35, John Wong, Endcaps, 40282-5, TARGET BOAT, Done, Sintering Ta-coated endcaps (temp measured)
|
Thursday, September 25, 2014, 17:32
Target boat is filled with Ta-coated endcaps. The caps are stacked together. In between each cap, a piece of graphite foil is used for separation so the Ta caps would not fused.
See link for photos:
https://www.dropbox.com/sh/rydtdho6ggh4l3l/AAAYmvqT0mVQ_pnz4iecS4ksa?dl=0
The boat is wrapped with 3-layers of heatshields. The chamber is currently being pumped down.
TGHT will be ramped up to 580A and the temperature will be measured.
Monday, September 29, 2014, 11:12
TGHt was stepped up to 40A on last Friday and chamber continues to pump down over the weekend.
Vac @ 2.56e-6 Torr, mp @ 19mTorr.
Ramping up TGHT 580A at 1.0A/min.
Monday, September 29, 2014, 11:50
TGHT tripped off at 53A. Reduce ramping rate to 0.5A/min for now.
Monday, September 29, 2014, 16:17
Vacuum is coming down to 9.5e-7 Torr. Increased ramping rate to 1.0A/min.
Tuesday, September 30, 2014, 11:59
TGHT reached to 580A/10.18V. Target has been heated at that current for almost 12 hrs. Vac @ 4.9e-7 Torr.
Local temp measured with Mikron = (1500C + 250 C correction) = 1750C
Cooling down at 2A/min.
Thursday, October 02, 2014, 11:13
The coating is fully sintered; no sign of any damage on the endcaps.
Process is successful.
|
Tuesday, September 23, 2014, 15:02, Laura Lambert, Empty, 40282-5, TARGET BOAT, In progress, Sintering Ta target boat with TaC coating
|
Tuesday, September 23, 2014, 15:00
A new target boat [new design with no end caps] was sprayed with TaC coating and let dry.
The target boat is wrapped with 3-layers of Ta-heat shield.
The boat was installed in EVAP2, chamber is currently being pumped down.
|
Tuesday, September 23, 2014, 18:32, John Wong, Empty, 40282-5, TARGET BOAT, Done, Sintering Ta target boat with TaC coating (with Temp measurement)
|
Laura Lambert wrote: |
Tuesday, September 23, 2014, 15:00
A new target boat [new design with no end caps] was sprayed with TaC coating and let dry.
The target boat is wrapped with 3-layers of Ta-heat shield.
The boat was installed in EVAP2, chamber is currently being pumped down.
|
Tuesday, September 23, 2014, 18:31
Chamber was pumped down to 2.5e-6 Torr.
HS water valve open; no leaks detected.
Stepping up TGHT to 40A - pressure is increasing...
Tuesday, September 23, 2014, 19:05
Auto-ramping TGHT to 580A at 0.5A/min. Temperature will be measured and TGHt will be adjusted accordingly.
Wednesday, September 24, 2014, 11:57
Pressure is stable at 2.2-6 Torr as TGHT is ramping up. Increase ramping rate to 2.0A/min. Currently TGHT at 540A.
Wednesday, September 24, 2014, 15:36
TGHT at 580A for 2 hrs. Inner tube temp (left side wall, viewing from the window port) ~1800C (measured with Mikron = 1550C +250C em. correction); Vac @ 1.67e-6 Torr.
Temperature measurement distance from the window to Mikron = 45cm.
Increase TGHT to reach 2000C (Mikron @ 1750C)
Wednesday, September 24, 2014, 18:14
TGHT has gone up to 725A/13.2V. Temp measured at 1740C (+250C = ~2000C). Pressure gone up to 5.5e-6 Torr and it's coming down slowly.
Will continue heating at this temperature for a few hours; then cool down afterward.
Wednesday, September 24, 2014, 18:56
Temperature is pretty stable at 1740C on Mikron, and pressure is still coming down, currently at 2.9e-6 Torr.
Slow ramping down TGHT at 1.0A/min. The chamber should be ready for venting tomorrow.
Target boat will be inspected.
Thursday, September 25, 2014, 17:25.
The boat was inspected and it turned out great! The coating was fully sintered and there is no sign of damage on the boat.
See the link for photos.
https://www.dropbox.com/sh/m7ycqhkj4avfull/AABHVTweTsP4ajeWZ6uoY010a?dl=0
|
Thursday, September 11, 2014, 14:23, Laura Lambert, , 40282-3, TARGET BOAT, Failed, Sintering TaC coated end caps
|
Thursday, September 11, 2014, 13:14
The target container end caps were coated with TaC spray and let dry.
The caps are inserted in the target boat wrapped in graphite foil with 3 x Ta-heat shields.
The chamber is currently pumping down.
Friday, September 12, 2014, 14:17
Chamber was pumped down overnight.
HS cooling water valves opened, no leaks detected.
IGP1 = 7.2e-7 Torr.
TGHT stepped up to 35A, TBHT at 0A.
Waited ~30min, current stabilized, vacuum started to drop, auto-ramp initiated at 0.2A/min.
Will ramp TGHT to 580A with a max 10V.
Good vacuum: 3.00e-5 Torr; Bad vacuum: 4.00e-5 Torr.
Monday, September 15, 2014, 11:31
TGHT stopped at 500A due to not high enough voltage max.
Increased max voltage to 12V
Monday, September 15, 2014, 14:17
IGP1 = 6.3e-7 Torr
Increasing ramping rate to 1.0A/min
Tuesday, September 16, 2014, 09:04
TGHT reached 577A and finished auto-ramping, then proceeded to drop down to 560A overnight.
Increased max voltage to 13.05A and TGHT to 580A.
Tuesday, September 16, 2014, 13:52
TGHT reached 580A and sat there for ~5hrs.
IGP1 = 6.1e-7 Torr.
Initiating auto-cool at 2.0A/min.
Wednesday, September 17, 2014, 13:03
Vented in air.
Opened up....looked 'deceivingly' ok.
then i took a layer of Ta off....grrrr
the 1st layer of Ta was holding the boat together. as soon as that layer was taken off the target boat broke.
see attached photos.
|
Wednesday, August 06, 2014, 16:10, John Wong, Ta, 38817-9, HP-SIS, In progress, Conditioning Ta target
|
Wednesday, August 06, 2014, 15:59
Target consists of 400 Ta discs.
Total packed length 4.5cm
Total mass 47.490g.
Re foil inserted.
Wednesday, August 06, 2014, 16:07
Chamber is currently being pumped down.
No Ta heat-shield wrapped (Want to check the temperature without it)
One end-cap inserted on left (wrt ionizer into the page).
TGHT and TBHT will be ramped up to 820A/230A at 2A/min.
Wednesday, August 06, 2014, 18:07
Vacuum at 2.3e-6 Torr. HS water valve opened. No leaks.
Initiated auto-ramping.
Thursday, August 07, 2014, 11:39
Target has been heated for 11hrs at TGHT/TBHT = 820A/230A.
Temperature measured with pyrometer:
Target leg = 1600C + (250 correction for e=0.25) = 1850C
Inside target material = dark, temp can't be measured.
Cooling down at 2A/min for TGHT and 1A/min TBHT.
|
Friday, August 08, 2014, 15:16, Laura Lambert, Ta, 38817-9, HP-SIS, Done, Conditioning Ta target
|
John Wong wrote: |
Wednesday, August 06, 2014, 15:59
Target consists of 400 Ta discs.
Total packed length 4.5cm
Total mass 47.490g.
Re foil inserted.
Wednesday, August 06, 2014, 16:07
Chamber is currently being pumped down.
No Ta heat-shield wrapped (Want to check the temperature without it)
One end-cap inserted on left (wrt ionizer into the page).
TGHT and TBHT will be ramped up to 820A/230A at 2A/min.
Wednesday, August 06, 2014, 18:07
Vacuum at 2.3e-6 Torr. HS water valve opened. No leaks.
Initiated auto-ramping.
Thursday, August 07, 2014, 11:39
Target has been heated for 11hrs at TGHT/TBHT = 820A/230A.
Temperature measured with pyrometer:
Target leg = 1600C + (250 correction for e=0.25) = 1850C
Inside target material = dark, temp can't be measured.
Cooling down at 2A/min for TGHT and 1A/min TBHT.
|
Friday, August 08, 2014, 15:14
Vented in air and opened up up this morning.
Endcaps inserted and expanded.
Rh foil and salts added.
|
Tuesday, August 05, 2014, 13:13, Laura Lambert, Empty, , TARGET BOAT, In progress, Sintering TaC coated end caps
|
Tuesday, August 05, 2014, 12:02
The target container end caps were coated with TaC spray and let dry.
The caps are inserted in the target boat vertically, wrapped in graphite foil with 3 x Ta-heat shield. [see attached photo]
The chamber is currently being pumped down.
|
Tuesday, August 05, 2014, 17:20, John Wong, , , TARGET BOAT, In progress, Sintering TaC coated end caps
|
Laura Lambert wrote: |
Tuesday, August 05, 2014, 12:02
The target container end caps were coated with TaC spray and let dry.
The caps are inserted in the target boat vertically, wrapped in graphite foil with 3 x Ta-heat shield. [see attached photo]
The chamber is currently being pumped down.
|
Tuesday, August 05, 2014, 17:19
HS water valve opened; no leaks detected.
Pressure @ 2.5e-6 Torr.
Ramping up TGHT to 580A @ 1A/min.
|
Thursday, August 07, 2014, 10:13, Laura Lambert, , , TARGET BOAT, Failed, Sintering TaC coated end caps
|
John Wong wrote: |
Laura Lambert wrote: |
Tuesday, August 05, 2014, 12:02
The target container end caps were coated with TaC spray and let dry.
The caps are inserted in the target boat vertically, wrapped in graphite foil with 3 x Ta-heat shield. [see attached photo]
The chamber is currently being pumped down.
|
Tuesday, August 05, 2014, 17:19
HS water valve opened; no leaks detected.
Pressure @ 2.5e-6 Torr.
Ramping up TGHT to 580A @ 1A/min.
|
Thursday, August 07, 2014, 08:11
Yesterday the target boat was taken out.
The boat broke as it turns out it was used for a Niobium target and therefore wasn't coated with TaC.
The end caps were fully sintered.
|
Friday, August 01, 2014, 13:27, Peter Kunz , , 40282-3, LP-SIS, In progress, ZrC #6 conditioning
|
Target was conditioned for 4 hours at 580A.
Initiating ramp-down sequence @ 2A/min
|
Tuesday, August 05, 2014, 12:01, Laura Lambert, , 40282-3, LP-SIS, Done, ZrC #6 conditioning
|
Peter Kunz wrote: |
Target was conditioned for 4 hours at 580A.
Initiating ramp-down sequence @ 2A/min
|
Tuesday, August 05, 2014, 12:00
target vented in air and taken out this morning
|
Friday, August 01, 2014, 11:47, Peter Kunz , , 40282-3, LP-SIS, In progress, ZrC #6 conditioning
|
The maximum current of 580A was reached at 9:15.
TGHT:RDCUR 578 A
TGHT:RDVOL 9.87 V
IGP1:RDVAC 3.8e-6
The temperature was measured with the Minolta 2-color pyrometer:
from the side - inside target container : ~1200 deg C
from the front trough hole in the heat shield : ~1800 deg C
|
Monday, July 28, 2014, 15:06, Laura Lambert, , 40282-3, LP-SIS, In progress, Sintering ZrC# 6 target
|
Monday, July 28, 2014, 14:41
Total number of foils: 445 discs
Total mass of materials [incl graphite foils]: 49.027 g
Total length packed: 11.2 cm
Container has no Ta heat shields.
Currently being pumped down.
|
Tuesday, July 29, 2014, 11:23, John Wong, , 40282-3, LP-SIS, In progress, Sintering ZrC# 6 target
|
Laura Lambert wrote: |
Monday, July 28, 2014, 14:41
Total number of foils: 445 discs
Total mass of materials [incl graphite foils]: 49.027 g
Total length packed: 11.2 cm
Container has no Ta heat shields.
Currently being pumped down.
|
Tuesday, July 29, 2014, 11:19
Chamber was pumped down overnight to ~5.5e-7 torr.
HS water valve opened; no leaks were detected.
Stepped up TGHT/TBHT to 40A. IG went up 8e-6 Torr and stabilized.
Initiated auto-ramping TGHT @ 580A, TBHt @ 230A at 0.2A/min
|
Wednesday, July 23, 2014, 15:07, John Wong, Empty, 40282-3, LP-SIS, In progress, Sintering TaC coated target container
|
Wednesday, July 23, 2014, 15:07
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min.
TBHT will be ramped up to 230A at 0.2A/min.
Chamber is currently being pumped down
Wednesday, July 23, 2014, 17:40
Vacuum came down to mid 10-6 Torr.
Stepped up TGHT and TBHT to 30A - IG1 @ 1.4e-5 Torr.
Initiated auto-ramping.
Thursday, July 24, 2014, 17:19
TGHT and TBHT have reached to 100A, and vacuum is coming down to 1.4e-6 Torr.
Increase ramping rate, TGHT to 1A/min, TBHT 0.5A/min.
Friday, July 25, 2014, 11:26
Target container temperature reaches ~1550C at 580A on TGHT and 230A TBHT, and it has been heated for ~10 hrs.
Auto-cooling initiated at 2A/min.
|
Monday, July 28, 2014, 10:52, Laura Lambert, Empty, 40282-3, LP-SIS, Done, Sintering TaC coated target container
|
John Wong wrote: |
Wednesday, July 23, 2014, 15:07
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min.
TBHT will be ramped up to 230A at 0.2A/min.
Chamber is currently being pumped down
Wednesday, July 23, 2014, 17:40
Vacuum came down to mid 10-6 Torr.
Stepped up TGHT and TBHT to 30A - IG1 @ 1.4e-5 Torr.
Initiated auto-ramping.
Thursday, July 24, 2014, 17:19
TGHT and TBHT have reached to 100A, and vacuum is coming down to 1.4e-6 Torr.
Increase ramping rate, TGHT to 1A/min, TBHT 0.5A/min.
Friday, July 25, 2014, 11:26
Target container temperature reaches ~1550C at 580A on TGHT and 230A TBHT, and it has been heated for ~10 hrs.
Auto-cooling initiated at 2A/min.
|
Monday, July 28, 2014, 10:50
vented in air and opened this morning. successful run
|
Friday, June 20, 2014, 12:01, Laura Lambert, SiC, 39530-8, HP-FEBIAD, In progress, Conditioning SiC#31 target
|
Friday, June 20, 2014, 11:14
Made from batch's: oct 23/2013, oct 31/2013 and june 2012
Total number of foils: 515 discs
Total mass of materials [incl graphite foils]: 64.7224g
Total length packed: 17.8cm
Container is wrapped with 3x Ta-heat shields.
Currently being pumped down.
Friday, June 20, 2014, 14:56
HS cooling water valves opened, no leaks detected.
IGP1 = 6.2e-6 Torr
TGHT max = 820A/ 17V
TBHT max = 300A/ 5V
Stepping up manually to 40A
Friday, June 20, 2014, 16:04
IGP1 = 8e-6 Torr
Slowly stepped up to 35A manually.
Vacuum has stabilized.
Initiating auto-ramp at 0.1A/min
|
Friday, June 20, 2014, 16:22, John Wong, SiC, 39530-8, HP-FEBIAD, In progress, Conditioning SiC#31 target
|
Laura Lambert wrote: |
Friday, June 20, 2014, 11:14
Total number of foils: 515 discs
Total mass of materials [incl graphite foils]: 64.7224g
Total length packed: 17.8cm
Container is wrapped with 3x Ta-heat shields.
Currently being pumped down.
Friday, June 20, 2014, 14:56
HS cooling water valves opened, no leaks detected.
IGP1 = 6.2e-6 Torr
TGHT max = 820A/ 17V
TBHT max = 300A/ 5V
Stepping up manually to 40A
Friday, June 20, 2014, 16:04
IGP1 = 8e-6 Torr
Slowly stepped up to 35A manually.
Vacuum has stabilized.
Initiating auto-ramp at 0.1A/min
|
Friday, June 20, 2014, 16:16
Changing the heating current...
From the previous SiC targets, TGHT was ramped up to 800A and yellow crystals were found; the end caps and target legs were also found broken (see my iPad). This might be too hot for the Ta-boat to handle the sintering process.
For this process,
TGHT will ramp up to 600A and TBHT to 230A over the weekend.
Then, the temperature will be measured. The sintering temperature of SiC is ~1800 - 2000C.
|
Monday, June 23, 2014, 09:47, Laura Lambert, SiC, 39530-8, HP-FEBIAD, In progress, Conditioning SiC#31 target
|
John Wong wrote: |
Laura Lambert wrote: |
Friday, June 20, 2014, 11:14
Total number of foils: 515 discs
Total mass of materials [incl graphite foils]: 64.7224g
Total length packed: 17.8cm
Container is wrapped with 3x Ta-heat shields.
Currently being pumped down.
Friday, June 20, 2014, 14:56
HS cooling water valves opened, no leaks detected.
IGP1 = 6.2e-6 Torr
TGHT max = 820A/ 17V
TBHT max = 300A/ 5V
Stepping up manually to 40A
Friday, June 20, 2014, 16:04
IGP1 = 8e-6 Torr
Slowly stepped up to 35A manually.
Vacuum has stabilized.
Initiating auto-ramp at 0.1A/min
|
Friday, June 20, 2014, 16:16
Changing the heating current...
From the previous SiC targets, TGHT was ramped up to 800A and yellow crystals were found; the end caps and target legs were also found broken (see my iPad). This might be too hot for the Ta-boat to handle the sintering process.
For this process,
TGHT will ramp up to 600A and TBHT to 230A over the weekend.
Then, the temperature will be measured. The sintering temperature of SiC is ~1800 - 2000C.
|
Monday, June 23, 2014, 09:45
IGP1 = 5e-6 Torr
TGHT and TBHT are at ~200A
Increasing ramping rate to 0.2A/min
Monday, June 23, 2014, 11:19
IGP1 = 6.9e-6 Torr
Increasing ramping rate to 2.0A/min
Monday, June 23, 2014, 12:09
JW: Pressure went up too fast... lower the TGHT ramping up rate to 1A/min.
Tuesday, June 24, 2014, 16:06
Increasing current with respect to temperature: See attached table
|
Tuesday, June 24, 2014, 23:57, John Wong, SiC, 39530-8, HP-FEBIAD, In progress, Conditioning SiC#31 target
|
Laura Lambert wrote: |
John Wong wrote: |
Laura Lambert wrote: |
Friday, June 20, 2014, 11:14
Total number of foils: 515 discs
Total mass of materials [incl graphite foils]: 64.7224g
Total length packed: 17.8cm
Container is wrapped with 3x Ta-heat shields.
Currently being pumped down.
Friday, June 20, 2014, 14:56
HS cooling water valves opened, no leaks detected.
IGP1 = 6.2e-6 Torr
TGHT max = 820A/ 17V
TBHT max = 300A/ 5V
Stepping up manually to 40A
Friday, June 20, 2014, 16:04
IGP1 = 8e-6 Torr
Slowly stepped up to 35A manually.
Vacuum has stabilized.
Initiating auto-ramp at 0.1A/min
|
Friday, June 20, 2014, 16:16
Changing the heating current...
From the previous SiC targets, TGHT was ramped up to 800A and yellow crystals were found; the end caps and target legs were also found broken (see my iPad). This might be too hot for the Ta-boat to handle the sintering process.
For this process,
TGHT will ramp up to 600A and TBHT to 230A over the weekend.
Then, the temperature will be measured. The sintering temperature of SiC is ~1800 - 2000C.
|
Monday, June 23, 2014, 09:45
IGP1 = 5e-6 Torr
TGHT and TBHT are at ~200A
Increasing ramping rate to 0.2A/min
Monday, June 23, 2014, 11:19
IGP1 = 6.9e-6 Torr
Increasing ramping rate to 2.0A/min
Monday, June 23, 2014, 12:09
JW: Pressure went up too fast... lower the TGHT ramping up rate to 1A/min.
Tuesday, June 24, 2014, 16:06
Increasing current with respect to temperature: See attached table
|
Tuesday, June 24, 2014, 23:44
Target has been heated at 600A. Local temperature measured on the right leg = 1814C.
RGA/ striptool/temperature data can be found on this link:
https://www.dropbox.com/sh/69memvh6fthodoz/AABZiSKAR9njhbqO4sBATVbla
Something interesting was observed about the out gassing of this target - the right window was coated when the temperature rose above 1500C (on the right end, could be hotter inside?) - see attachment.
I suspect this is Si vapour deposited on the window when the target heater got closed to the sintering temperature for SiC (1800 - 2000C).
Once the chamber is vented, the coated window will be inspected and analyzed. More details later...
Initiate auto-cooling (slow cool down) TGHT 1A/min; TBHT 0.5/min. Chamber should be able for venting tomorrow afternoon.
|
Tuesday, June 17, 2014, 13:20, Laura Lambert, Empty, 39530-8, HP-FEBIAD, Done, Sintering TaC coating container for SiC#30 part 2
|
Tuesday, June 17, 2014, 13:11
Target container is coated with TaC.
Container is wrapped with 3x Ta-heat shields.
Currently being pumped down.
For sintering process:
TGHT and TBHT will be ramped up to 820A and 300A respectively at 0.1A/min
Tuesday, June 17, 2014, 14:22
HS water cooling valves opened, no leaks detected.
IGP1 @1.8e-6 Torr
TGHT max = 820A/ 17V
TBHT max = 300A/ 5V
Stepped up manually to 40A, waited ~20min, vacuum stable.
Initiating auto-ramp @ 1.0A/min
Wednesday, June 18, 2014, 11:24
TGHT and TBHT reached their respective 820A and 300A last night.
Internal temp measured from side of EVAP2 with mikron = 1830C
IGP1 = 7.6e-7 Torr
Initiating auto-cool down process at 2.0A/min and 1.0A/min for TGHT and TBHT respectively
vented and opened this morning.
smooth run
|
Friday, June 13, 2014, 14:57, Laura Lambert, Ta, 40282-2, LP-SIS, In progress, Conditioning Ta#43 target
|
Friday, June 13, 2014, 14:53
Container is filled with 400 discs of Ta foils; target length = 5.2cm;
Total mass ( Ta foils + wire) = 45.92g
No Ta foil heat shield.
No caps inserted.
Chamber pumped down this morning.
HS cooling water valves opened, no leaks detected.
IG @ 5.8e-6 Torr.
TGHT max = 580A
TBHT max = 230A
Ramping rate 0.2A/min.
Monday, June 16, 2014, 11:46
TGHT and TBHT reached their respective 580A and 230A over the weekend.
IGP1 currently at 3.2e-7 Torr.
Internal temp [measured using mikron, right side of EVAP2, pointed at discs inside] = 1375C
|
Monday, June 16, 2014, 17:42, John Wong, Ta, 40282-2, LP-SIS, In progress, Conditioning Ta#43 target
|
Laura Lambert wrote: |
Friday, June 13, 2014, 14:53
Container is filled with 400 discs of Ta foils.
No Ta foil heat shield.
No caps inserted.
Chamber pumped down this morning.
HS cooling water valves opened, no leaks detected.
IG @ 5.8e-6 Torr.
TGHT max = 580A
TBHT max = 230A
Ramping rate 0.2A/min.
Monday, June 16, 2014, 11:46
TGHT and TBHT reached their respective 580A and 230A over the weekend.
IGP1 currently at 3.2e-7 Torr.
Internal temp [measured using mikron, right side of EVAP2, pointed at discs inside] = 1375C
|
Monday, June 16, 2014, 17:21
Further stepping up TGHT to 650A.
Temperature measured on target discs = 1542C. Vac @ 3.28e-7 Torr.
Initiate cooling down process; 2A/min for TGHT; 1A/min for TBHT
|
Tuesday, June 17, 2014, 10:14, Laura Lambert, Ta, 40282-2, LP-SIS, Done, Conditioning Ta#43 target
|
John Wong wrote: |
Laura Lambert wrote: |
Friday, June 13, 2014, 14:53
Container is filled with 400 discs of Ta foils.
No Ta foil heat shield.
No caps inserted.
Chamber pumped down this morning.
HS cooling water valves opened, no leaks detected.
IG @ 5.8e-6 Torr.
TGHT max = 580A
TBHT max = 230A
Ramping rate 0.2A/min.
Monday, June 16, 2014, 11:46
TGHT and TBHT reached their respective 580A and 230A over the weekend.
IGP1 currently at 3.2e-7 Torr.
Internal temp [measured using mikron, right side of EVAP2, pointed at discs inside] = 1375C
|
Monday, June 16, 2014, 17:21
Further stepping up TGHT to 650A.
Temperature measured on target discs = 1542C. Vac @ 3.28e-7 Torr.
Initiate cooling down process; 2A/min for TGHT; 1A/min for TBHT
|
Tuesday, June 17, 2014, 10:08
TGHT and TBHT reached 0A last night.
Turned off EVAP2
Venting chamber
Process Complete
|
Monday, June 09, 2014, 17:15, Cameron Hodgins, , , TARGET BOAT, In progress, Sintering several carbides on tantalum foil backing
|
Target boat is now being cooled at 1 A/min from the starting point (616 A) down to 0 A. |
Monday, June 09, 2014, 13:56, Cameron Hodgins, , , TARGET BOAT, In progress, Sintering several carbides on tantalum foil backing
|
Manually changed current from 500 to 615 A, monitoring the temperature. Temperature went from 1657 C up to 1838 C. Pressure increased up to 7.2e-7 T. Samples should be left for about 4 hours (615 A started just before 13:00), then the goal is to ramp current back to zero. |
Friday, June 06, 2014, 16:01, Cameron Hodgins, , , TARGET BOAT, In progress, Sintering several carbides on tantalum foil backing
|
Auto-ramp started. Max current = 500 A, voltage = 11.05 V. Current is being increased at 2 A/min. In the first 20 minutes, the pressure went up to about 10E-6 T, but has slowly decreased since then. Everything looks ok. The system will be left until Monday morning (June 9th). |
Friday, May 30, 2014, 13:15, Cameron Hodgins, , , , In progress, Sintering several carbides on tantalum foil backing
|
Pressure down to 7.1e-7 Torr. Water valve to heat shield was opened; pressure remained stable.
Current turned up to 40 A for now. Will increase at 2 A/min up to 500 A over the weekend, then on Monday we will turn it up to 600 A and check the temperature. |
Thursday, May 29, 2014, 18:16, Cameron Hodgins, , , TARGET BOAT, In progress, Sintering several carbides on tantalum foil backing
|
Purpose: Sinter one sample of each of TiC, VC, Cr3C2, ZrC, NbC, Mo2C, TaC, and WC on 5x10 mm tantalum foil to see if the samples are usable for SEM.
Samples were prepared using a solution of PEG (2.56 g), PVB (2.45 g), paraffin oil (1.12 g), MEK (15 mL), and EtOH (23 mL). Slurries made using 0.0013 mol of each carbide with ~230 uL of the solution. Applied via paintbrush onto 5x10 mm tantalum foil.
The samples were placed directly on the target boat, no graphite layer between. We will check to see if the tantalum foil fuses to the boat or not.
Currently (May 29th), the chamber is still pumping down. John and I will continue the procedure tomorrow.
|
Thursday, April 24, 2014, 18:13, John Wong, , , TARGET BOAT, Done, Tests: Sintering carbon Mesh coated with WC
|
Thursday, April 24, 2014, 17:25
The purpose of this experiment is to see if the carbon mesh is suitable for coating and sintering with uranium carbide. For this test, the mesh is coated with WC slurry (previously prepared).
The carbon mesh disks are bought from ERG aerospace corporation; the specifications of the mesh can be found on the link: http://www.ergaerospace.com/RVC-properties.htm
Photos, EDX, SEM, RGA, etc... and be found on this link: https://www.dropbox.com/sh/6ic932wu8yl9ad2/7rHFTiSzLY
Thursday, April 24, 2014, 17:51
TEST #1: Carbon Mesh, WC - RF sputtered - Then WC coated and sintered.
Target boat is loaded with a piece of WC coated carbon mesh (1/4 size cut out with the laser cutter). Chamber is pumping down, currently at 3.2e-6 Torr.
HS water valve open - no leaks are detected.
TGHT will be ramped up to 500A at 1.0A/min.
RGA is running.
Material temp will be measured...
Monday, May 05, 2014, 17:35
Test #1:
TGHT was ramped up to 680A/13.77V. Vacuum was at 1.62e-6 Torr (and coming down). Carbon mesh was heated up to 1900C. See the link to the dropbox above for more results.
Monday, May 05, 2014, 17:39
Test #2: Carbon mesh (pure) coated with WC - then sintered.
Chamber has been pumped down to 3.5 e-6 Torr.
Sample will be heated up to 500A at 1.0A/min. (Then step up to 680A while monitoring the vacuum).
RGA is running.
Wednesday, May 07, 2014, 14:36
Observations:
TGHT was at 650A/12.96V for 6 hrs and temperature was measured at 1930C.
At some point after that (~20:40hr on May 6), the voltage went up to 14.77V (current remained constant at 650A), the temp went up 2110C - for only about 45 minute before the voltage dropped
back down to 12.53V and the temperature ~1800C. Is the boat creaking more??? There were a few crack lines on the boat after Test#1.
Today, TGHT was raised up to 725A and after an hour at that current the temperature was measured at 1930A.
Now, at Wednesday, May 07, 2014, 14:47 - Lowered the current back to 685A/13.78V - temperature measured at 1900C.
One thing to note... the vacuum is showing a lot of spikes but remains at around 7.5e-7 Torr.
The RGA/Current/Voltage/Temp can be found here: https://www.dropbox.com/sh/1yaa7ez3nydl67m/8v4ZRT2slq
Thursday, May 29, 2014, 16:56
The process is done. Chamber was vented...
|
Thursday, March 27, 2014, 18:04, John Wong, , , TARGET BOAT, In progress, Studying WC sintering on Ta surface
|
Thursday, March 27, 2014, 17:38
TEST #1
WC slurry was prepared in non-aqueous environment (see lab book for procedures). The solution was dripped on two Ta plates (3.1cm2) and let dry.
Another Ta plate (3.1 cm2) was sprayed with TaC coating (for comparison).
All 3 coated Ta plates are put in a target boat and the boat is wrapped with 3 layers of Ta-heat shields.
HS water valves open; no leaks detected.
TGHT will be ramped up to 700A at 2.0A/min.
RGA is running and gases are being monitored. See link:
https://www.dropbox.com/sh/625xl7zgepbybmu/GQJTlMo-5a
Friday, March 28, 2014, 09:13
TGHT reached to 700A and samples were heated up over night.
Cooling down Evap at 4A/min.
Tuesday, April 01, 2014, 17:37
Previous samples, namely WC#1, #2, TC#1 were fully sinterred. See above link for photos.
TEST#2
Samples WC#3, #4, #5 are sprayed coated with WC solution. Grains were pre-treated at 400RPM.
These 3 new samples are loaded in a boat, wrapped with 3 layers of Ta-heat shields.
Chamber is pumped down; no water leaks are detected.
TGHT will be ramped up to 700A at 2.0A/min
RGA is running.
Samples were analyzed with SEM/EDX. The results are inconclusive because W and Ta peaks are very close together. And WC coated layer may be even too thin to analyze.
Monday, April 14, 2014, 16:32
Test#3: Coated WC on Endcap. Total mass WC ~350mg.
Sintered at 500A/9.5V; measure temperature on actual sample surface ~1700C. Sample heated >24hr.
Cooling down TGHT at 2A/min. IG currently at 3.1e-7 Torr.
|
Friday, March 21, 2014, 16:18, John Wong, TiC, 38817-8, HP-SIS, In progress, Sintering TiC
|
Friday, March 21, 2014, 16:09
Target container is loaded with 360 Discs of TiC.
Target length = 11.7cm.
Total green mass = 40.945g
Container is wrapped with 3 Ta-heat shields, and have been pumped down in the chamber.
For the sintering process:
TGHT ramp up to 820A, and TGHT to 300A at 0.1A/min.
Friday, March 21, 2014, 16:15
TGHT/TBHT were manually stepped up to 40A.
Vac stabilizes at 1.7e-6 Torr.
Initiate auto-ramping...
|
Wednesday, March 26, 2014, 11:07, Laura Lambert, TiC, 38817-8, HP-SIS, In progress, Sintering TiC
|
John Wong wrote: |
Friday, March 21, 2014, 16:09
Target container is loaded with 360 Discs of TiC.
Target length = 11.7cm.
Total green mass = 40.945g
Container is wrapped with 3 Ta-heat shields, and have been pumped down in the chamber.
For the sintering process:
TGHT ramp up to 820A, and TGHT to 300A at 0.1A/min.
Friday, March 21, 2014, 16:15
TGHT/TBHT were manually stepped up to 40A.
Vac stabilizes at 1.7e-6 Torr.
Initiate auto-ramping...
|
Wednesday, March 26, 2014, 11:05
TBHT reached max desired current of 300A
IGP1 = 1.4e-6 Torr
TGHT = 543A
Increasing TGHT auto-ramp to 2.0A/min
|
Wednesday, March 26, 2014, 18:23, John Wong, TiC, 38817-8, HP-SIS, Done, Sintering TiC#4
|
Laura Lambert wrote: |
John Wong wrote: |
Friday, March 21, 2014, 16:09
Target container is loaded with 360 Discs of TiC.
Target length = 11.7cm.
Total green mass = 40.945g
Container is wrapped with 3 Ta-heat shields, and have been pumped down in the chamber.
For the sintering process:
TGHT ramp up to 820A, and TGHT to 300A at 0.1A/min.
Friday, March 21, 2014, 16:15
TGHT/TBHT were manually stepped up to 40A.
Vac stabilizes at 1.7e-6 Torr.
Initiate auto-ramping...
|
Wednesday, March 26, 2014, 11:05
TBHT reached max desired current of 300A
IGP1 = 1.4e-6 Torr
TGHT = 543A
Increasing TGHT auto-ramp to 2.0A/min
|
Wednesday, March 26, 2014, 18:18
TGHT has reached to 820A\13.4V and target has been heated at that current for 4.5 hours.
Vac is coming down to 1.1e-6 Torr.
See link for RGA results: https://www.dropbox.com/sh/08dcxskux21aqap/1SF_dTJB4l
Cooling down in process at 2A/min for TGHT and 1A/min for TBHT.
Thursday, March 27, 2014, 11:14
Target is cooled down. TGHT/TBHT have reached to 0A.
All pumps off; chamber will be vented soon.
Friday, March 28, 2014, 15:00
Target has been assembled. Heat shield WO#39956-10
|
Monday, March 10, 2014, 11:52, John Wong, , , , Problems resolved, The Chiller is down
|
Monday, March 10, 2014, 11:45
The chiller tripped off on March 7, 2014.
- Water is not flowing into the chiller; paddle wheel shows no signal.
- Tried turning on the chiller locally; a few seconds later, it tripped off.
- Motor is not responding;
- EPICS is not responding;
- All other water flow signals to TGHT, TBHT, HS, are responding;
Continue investigating...
Monday, March 10, 2014, 14:36
The water line to the chiller is disconnected, and is re-connected straight to the TGHT power supply. The paddle wheel is responding - the cooling line in the power supply is not blocked.
It is confirmed the chiller is broken.
Will discuss if we can use the Evaporator without a chiller but with the DI water connected directly to the TGHT power supply....
Friday, March 14, 2014, 14:50
The chiller was replaced with a "new" one.
Checked the chiller interlock - It's working.
The evaporator is now operational.
Friday, March 21, 2014, 16:19
Note about Auto-ramping program.
Previously the auto-rampiong program takes the Chiller as part of the reference to the interlocks. Because the New chiller is not connected to EPICS; all the references to the Chiller on the auto-ramping program has been removed in order for it to function.
|
Monday, March 10, 2014, 11:45, John Wong, , , , Maintenance, Replaced Backing Pump hose
|
Monday, March 10, 2014, 11:44
Rick replaced the backing pump hose from 1.5" to 2.0" for better flow. And the HEPA filter was checked - it looks OK.
|
Friday, March 07, 2014, 11:46, Laura Lambert, , 40282-3, TARGET BOAT, In progress, Sintering TaC coated end caps
|
Friday, March 07, 2014, 11:41
The target container end-caps were sintered previously, but did not fully complete the sintering process [See elog entry # 119 EVAP2]
The caps are inserted in the target boat wrapped in graphite foils with 3 x Ta-heat shields.
The chamber was pumped down overnight.
IGP1 = 2e-7 Torr
HS cooling water valves were opened; no leaks detected.
TGHT was stepped up to 35A, voltage max set at 9.05V. TBHT currently at 0A.
Friday, March 07, 2014, 11:52
Waited ~20min, current stabilized, vacuum started to drop, auto-ramp initiated at 0.5A/min and max setpoint to 500A.
Will ramp to 500A due to last failed round of end caps breaking with 3-ta heat shields at 580A.
Good vacuum: 3.00e-5 Torr; Bad vacuum: 4.00e-5 Torr.
Friday, March 07, 2014, 13:21
IGP1 = 8e-7 Torr.
TGHT = 72A
Vacuum stable; therefore, increasing ramping rate up to 1.0A/min
Friday, March 07, 2014, 14:20
IGP1 = 9.8e-7 Torr
TGHT = 130A
Vacuum stable; therefore, increasing ramping rate up to 2.0A/min
|
Friday, March 07, 2014, 22:25, John Wong, , 40282-3, TARGET BOAT, Problems, Sintering TaC coated end caps
|
Laura Lambert wrote: |
Friday, March 07, 2014, 11:41
The target container end-caps were sintered previously, but did not fully complete the sintering process [See elog entry # 119 EVAP2]
The caps are inserted in the target boat wrapped in graphite foils with 3 x Ta-heat shields.
The chamber was pumped down overnight.
IGP1 = 2e-7 Torr
HS cooling water valves were opened; no leaks detected.
TGHT was stepped up to 35A, voltage max set at 9.05V. TBHT currently at 0A.
Friday, March 07, 2014, 11:52
Waited ~20min, current stabilized, vacuum started to drop, auto-ramp initiated at 0.5A/min and max setpoint to 500A.
Will ramp to 500A due to last failed round of end caps breaking with 3-ta heat shields at 580A.
Good vacuum: 3.00e-5 Torr; Bad vacuum: 4.00e-5 Torr.
Friday, March 07, 2014, 13:21
IGP1 = 8e-7 Torr.
TGHT = 72A
Vacuum stable; therefore, increasing ramping rate up to 1.0A/min
Friday, March 07, 2014, 14:20
IGP1 = 9.8e-7 Torr
TGHT = 130A
Vacuum stable; therefore, increasing ramping rate up to 2.0A/min
|
Friday, March 07, 2014, 22:22
Target current was at 500A before it tripped off on the chiller. Tried to reset the chiller but to no avail. Don't know what is going on yet.
The TGHT/TBHT cooling water is still on, and this should OK while the HOT target boat is cooling down at the moment.
Will leave it for now and further investigate on Monday
|
Friday, March 07, 2014, 10:34, Anders Mjos, , , , Problems resolved, TGHT2 water flow signal
|
There was no signal going from the coils to the PLC. After manipulating the connection points on the coil a signal could again be established. Frequency is ~ 40Hz. |
Tuesday, February 25, 2014, 16:10, Laura Lambert, , 40282-3, TARGET BOAT, Done, Sintering TaC coated end caps
|
Tuesday, February 25, 2014, 16:08
The target containers end-caps were coated with TaC spray and let dry.
The caps are inserted in the target boat vertically with no heat shield and no graphite foil. [see attached photo]
The chamber is currently being pumped down overnight.
Wednesday, February 26, 2014, 09:54
Chamber was pumped down overnight to 4.2e-7 Torr.
HS cooling water valves opened; no leaks detected.
TGHT was stepped up to 35A, voltage max set at 14V. TBHT currently at 0A.
Waited ~20min, current stabilized, vacuum started to drop, auto-ramp initiated at 0.2A/min and max setpoint to 700A.
Will ramp up to 700A rather than the usual 580A due to last round of endcaps not fully sintering at 580A with new target boat design.
Good vacuum: 3.00e-5 Torr; Bad vacuum: 4.00e-5 Torr.
Thursday, February 27, 2014, 09:38
TGHT has been slowly ramping up overnight at a rate of 0.2A/min.
IGP1 = 2.8e-7 Torr; TGHT = 311A, 4.3V
Stepping ramping rate up to 2.0A/min.
Friday, February 28, 2014, 08:53
TGHT reached max setpoint of 700A yesterday evening.
Internal temp measured with Mikron = 1700C
IGP1 = 3e-7 Torr
Power = 12.95V
Initiating auto-cooling at 2.0A/min.
Monday, March 03, 2014, 11:46
Vented and opened chamber this morning.
End caps not fully sintered!
See attached photo comparison of fully sintered [grey], partially sintered from this round [light green] and pre-sinter [dark green].
Will not bother re-sintering, as partial sinter is enough.
|
Tuesday, February 18, 2014, 12:19, Laura Lambert, Empty, 40282-3, TARGET BOAT, Done, Sintering Ta target boat with TaC coating
|
Tuesday, February 18, 2014, 12:12
A new target boat was sprayed with TaC coating and let dry.
The target boat is NOT wrapped with Ta-heat shield.
Thermocouples have been attached to the target boat in order to monitor the internal temperature of the new target boat design.
The boat was installed in Evap#2, chamber is currently being pumped down.
Tuesday, February 18, 2014, 14:20
Chamber was pumped down this morning to 2.9e-6 Torr. HS cooling water valves were opened, no leaks detected.
TGHT was stepped up to 35A, voltage max set at 14V. TBHT currently at 0A.
Waited ~20min, current stabilized, vacuum started to drop, auto-ramp initiated at 0.2A/min and max setpoint to 700A.
Good vacuum: 3.00e-5 Torr; Bad vacuum: 4.00e-5 Torr.
Temperature reading on left: thermocouple touching edge of target boat; temperature reading on right: thermocouple floating in center of target boat.
Wednesday, February 19, 2014, 09:11
TGHT has been slowly ramping up overnight at a rate of 0.2A/min
IGP1 = 3.9e-7 Torr, TGHT = 260A; stepping ramping rate up to 2.0A/min
Wednesday, February 19, 2014, 15:25
IGP1 = 9.4e-7 Torr
Thermocouple T2 = 1267.8C
Internal temp measured with Mikron = 1600C
Increasing max setpoint to 720A due to previous not fully sintered new design of target boat.
Thursday, February 20, 2014, 09:17
Thermocouple T2 = 1254.5C
Internal temp measured with Mikron = 1811C
IGP1 = 2.6e-7 Torr
Reached max setpoint yesterday evening.
Initiating auto-cooling at 2.0A/min.
Friday, February 21, 2014, 10:47
Vented and opened chamber this morning.
Target boat not fully sintered. [see attached photos]
Close to a full sinter, and will re-sinter next week with endcaps, so will not re-sinter by itself.
|
Tuesday, February 11, 2014, 13:49, Laura Lambert, Empty, 38817-8, HP-SIS, Done, Sintering TaC coating container for TiC
|
Tuesday, February 11, 2014, 13:43
Target container is coated with TaC and wrapped with 3-Ta heat shields.
TGHT and TBHT will be ramped up to 820A and 300A, respectively.
Ramping rate set to 0.2A/min.
Good vac = 3e-5 Torr, Bad vac = 4e-5 Torr.
Chamber currently being pumped down...
Tuesday, February 11, 2014, 16:33
Chamber pumped down to 2e-6 Torr.
HS cooling water valves opened; no leaks detected.
Will step up in the a.m.
Wednesday, February 12, 2014, 11:41
IGP1 = 1.5e-7 Torr
TGHT max voltage = 17.05V, TBHT max voltage = 5V
Stepped TGHT and TBHT up to 35A
Waited 1hr15 before vacuum stabilized/ started to drop.
Initiating auto-ramping.
Thursday, February 13, 2014, 10:19
TBHT and TGHT have both reached 300A
IGP1 = 2.4e-7 Torr.
Increasing TGHT auto-ramp to 2.0A/min
Friday, February 14, 2014, 08:58
TGHT reached 820A yesterday afternoon. Measured internal temp this morning at 1300C.
Initiated TGHT auto-cooling at 2.0A/min and TBHT at 1.0A/min.
IGP1 = 3.2e-7 Torr.
Monday, February 17, 2014, 12:02
Cooled down friday. Vented this morning.
Container fully sintered, smooth run!
|
Friday, January 31, 2014, 12:10, Laura Lambert, Empty, 39165-10, LP-SIS, Done, Sintering TaC coating container for Ta?
|
Friday, January 31, 2014, 11:28
Target container is coated with TaC.
The container is wrapped with 3 x Ta heat-shield.
Chamber was pumped down to 1.9e-7 Torr.
HS water valves were opened, no leak detected.
TGHT and TBHT were stepped up to 35A. Waited ~20min, current stabilized and vacuum starting to drop.
TGHT will be ramped up to 580A at 0.2A/min, max voltage = 11.05V.
TBHT will be ramped up to 230A at 0.2A/min, max volatge = 5V.
Initiating auto-ramping: Good Vac = 3.0e-5 Torr, Bad Vac = 4.0e-5 Torr.
Monday, February 03, 2014, 10:21
TGHT reached 580A pver the weekend.
TBHT sitting at 1.4A, checked archive: never went over 1.6A. Aborted auto-ramp, re-starting auto ramp process for TBHT.
IGP1 = 1.6e-7 Torr.
Monday, February 03, 2014, 15:23
TBHT running smoothly, must have been and electrical problem.
TBHT currently at 85A, vacuum has not changed, increasing TBHT auto-ramp to 2.0A/min
Tuesday, February 04, 2014, 10:10
TBHT reached 230A yesterday pm. Measured temp this morning at 1800C.
Initiated TGHT/TBHT auto-cooling at 2.0A/min.
Wednesday, February 05, 2014, 11:33
Chamber cooled down overnight, vented and opened up this morning.
Smooth run! Container fully sintered.
|
Tuesday, January 28, 2014, 15:46, Laura Lambert, , 40282-4, TARGET BOAT, Failed, Sintering TaC coated end caps
|
Tuesday, January 28, 2014, 15:43
The target containers end-caps were coated with TaC spray and let dry.
Each cap is wrapped with a small piece of graphite foil and inserted in the target boat. [see attached photo]
The chamber is currently being pumped down overnight.
Wednesday, January 29, 2014, 11:32
Chamber was pumped down to 1.6e-7 Torr overnight.
HS cooling water valve opened; no leaks detected.
TGHT was stepped up to 35A, voltage max set at 11.05V. TBHT currently at 0A.
Waited ~20min, current stabilized, vacuum started to drop, auto-ramp initiated at 0.2A/min and max setpoint to 580A.
Good vacuum: 3.00e-5 Torr, Bad vacuum 4.00e-5 Torr.
Thursday, January 30, 2014, 09:06
TGHT has been slowly ramping up overnight at a rate of 0.2A/min.
IGP1 = 2.4e-7 Torr, TGHT = 283A; stepping ramping rate up to 2.0A/min.
Thursday, January 30, 2014, 15:53
TGHT reached 580A at 11:45. Measured temp @1650C.
Initiating TGHT auto-cooling now at 2.0A/min.
Friday, January 31, 2014, 09:04
Chamber cooled down overnight, vented and opened this morning.
Smooth run!
Friday, January 31, 2014, 11:21
Opened up the end caps, turns out it wasn't such a smooth run...they're not fully sintered
See attached photo comparison between fully sintered end cap [silver] and end cap from this run [green].
Will re-install and re-sinter next week.
Wednesday, February 05, 2014, 11:34
End-caps re-installed into EVAP2
Target boat is wrapped with 3 x Ta heat-shield.
Chamber is currently being pumped down.
Wednesday, February 05, 2014, 14:31
Chamber was pumped down to 5e-7 Torr this morning.
HS cooling water valve opened, no leaks detected.
TGHT was stepped up to 35A, voltage max set at 11.05V. TBHT currently at 0A.
Waited ~20min, current stabilized, vacuum started to drop, auto-ramp initiated at 0.2A/min and max setpoint to 580A.
Good Vacuum: 3.00e-5 Torr, Bad vacuum 4.00e-5 Torr.
Thursday, February 06, 2014, 09:06
TGHT has been slowly ramping up overnight at a rate of 0.2A/min.
IGP1 = 1.1e-7 Torr, TGHT = 259A; stepping ramping rate up to 2.0A/min.
Friday, February 07, 2014, 10:10
TGHT reached 580A yesterday. Measured internal temp @ 1500C.
Initiated TGHT auto-cooling this morning at 2.0A/min
Tuesday, February 11, 2014, 13:30
Vented and opened chamber this morning.
Endcaps are toast [see pictures attached]
Some of the endcaps broke/fried, others deformed-none useable.
Possibly due to new target boat resulting in more current?
Too much heat with Ta heat shields?
Bad News Bears
|
Monday, January 20, 2014, 16:35, Laura Lambert, Empty, Ta-Target boat, , , Sintering Ta target boat with TaC coating
|
Monday, January 20, 2014, 16:32
A new target boat was sprayed with TaC coating and let dry this morning.
The target boat is NOT wrapped with Ta-heat shield.
The boat was installed in Evap#2, chamber is currently being pumped down overnight.
|
Tuesday, January 21, 2014, 11:33, Laura Lambert, Empty, 40282-4, TARGET BOAT, , Sintering Ta target boat with TaC coating
|
Laura Lambert wrote: |
Monday, January 20, 2014, 16:32
A new target boat was sprayed with TaC coating and let dry this morning.
The target boat is NOT wrapped with Ta-heat shield.
The boat was installed in Evap#2, chamber is currently being pumped down overnight.
|
Tuesday, January 21, 2014, 11:10
Chamber was pumped down to ~2e-7 Torr. HS cooling water valves were opened, no leaks detected.
TGHT was stepped up to 35A, voltage max set at 13V. TBHT currently @ 0A.
Waited ~20min, current stabilized, vacuum started to drop, auto-ramp initiated at 2.0A/min and max setpoint to 700A.
Good vacuum: 3.00e-5 Torr, Bad vacuum 4.00e-5 Torr.
|
Tuesday, January 21, 2014, 11:56, Laura Lambert, Empty, 40282-4, TARGET BOAT, , Sintering Ta target boat with TaC coating
|
Laura Lambert wrote: |
Laura Lambert wrote: |
Monday, January 20, 2014, 16:32
A new target boat was sprayed with TaC coating and let dry this morning.
The target boat is NOT wrapped with Ta-heat shield.
The boat was installed in Evap#2, chamber is currently being pumped down overnight.
|
Tuesday, January 21, 2014, 11:10
Chamber was pumped down to ~2e-7 Torr. HS cooling water valves were opened, no leaks detected.
TGHT was stepped up to 35A, voltage max set at 13V. TBHT currently @ 0A.
Waited ~20min, current stabilized, vacuum started to drop, auto-ramp initiated at 2.0A/min and max setpoint to 700A.
Good vacuum: 3.00e-5 Torr, Bad vacuum 4.00e-5 Torr.
|
Tuesday, January 21, 2014, 11:51
Vacuum was grumpy and was well on it's way to tripping off [reached 5e-5 Torr], auto ramping was stopped at ~95A and quickly stepped down to 90A to avoid tripping it off.
Allowed vacuum to settle back down to 2.3e-6 Torr. Auto ramping changed to 0.2A/min and re-started.
close-call!
|
Wednesday, January 22, 2014, 09:49, Laura Lambert, Empty, 40282-4, TARGET BOAT, , Sintering Ta target boat with TaC coating
|
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Monday, January 20, 2014, 16:32
A new target boat was sprayed with TaC coating and let dry this morning.
The target boat is NOT wrapped with Ta-heat shield.
The boat was installed in Evap#2, chamber is currently being pumped down overnight.
|
Tuesday, January 21, 2014, 11:10
Chamber was pumped down to ~2e-7 Torr. HS cooling water valves were opened, no leaks detected.
TGHT was stepped up to 35A, voltage max set at 13V. TBHT currently @ 0A.
Waited ~20min, current stabilized, vacuum started to drop, auto-ramp initiated at 2.0A/min and max setpoint to 700A.
Good vacuum: 3.00e-5 Torr, Bad vacuum 4.00e-5 Torr.
|
Tuesday, January 21, 2014, 11:51
Vacuum was grumpy and was well on it's way to tripping off [reached 5e-5 Torr], auto ramping was stopped at ~95A and quickly stepped down to 90A to avoid tripping it off.
Allowed vacuum to settle back down to 2.3e-6 Torr. Auto ramping changed to 0.2A/min and re-started.
close-call!
|
Wednesday, January 22, 2014, 09:46
TGHT has been slowly ramping up overnight at a rate of 0.2A/min.
IGP1 = 2.9e-7 Torr, TGHT = 342A; stepping ramping rate up to 2.0A/min.
|
Wednesday, January 22, 2014, 13:46, Laura Lambert, Empty, 40282-4, TARGET BOAT, , Sintering Ta target boat with TaC coating
|
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Monday, January 20, 2014, 16:32
A new target boat was sprayed with TaC coating and let dry this morning.
The target boat is NOT wrapped with Ta-heat shield.
The boat was installed in Evap#2, chamber is currently being pumped down overnight.
|
Tuesday, January 21, 2014, 11:10
Chamber was pumped down to ~2e-7 Torr. HS cooling water valves were opened, no leaks detected.
TGHT was stepped up to 35A, voltage max set at 13V. TBHT currently @ 0A.
Waited ~20min, current stabilized, vacuum started to drop, auto-ramp initiated at 2.0A/min and max setpoint to 700A.
Good vacuum: 3.00e-5 Torr, Bad vacuum 4.00e-5 Torr.
|
Tuesday, January 21, 2014, 11:51
Vacuum was grumpy and was well on it's way to tripping off [reached 5e-5 Torr], auto ramping was stopped at ~95A and quickly stepped down to 90A to avoid tripping it off.
Allowed vacuum to settle back down to 2.3e-6 Torr. Auto ramping changed to 0.2A/min and re-started.
close-call!
|
Wednesday, January 22, 2014, 09:46
TGHT has been slowly ramping up overnight at a rate of 0.2A/min.
IGP1 = 2.9e-7 Torr, TGHT = 342A; stepping ramping rate up to 2.0A/min.
|
Wednesday, January 22, 2014, 13:43
TGHT is sitting at 693A, IGP1 = 1.3e-6 Torr.
Stepping up TGHT voltage up to 14V from 13.05V to reach the max current of 700A.
|
Wednesday, January 22, 2014, 15:13, John Wong, Empty, 40282-4, TARGET BOAT, , Sintering Ta target boat with TaC coating
|
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Monday, January 20, 2014, 16:32
A new target boat was sprayed with TaC coating and let dry this morning.
The target boat is NOT wrapped with Ta-heat shield.
The boat was installed in Evap#2, chamber is currently being pumped down overnight.
|
Tuesday, January 21, 2014, 11:10
Chamber was pumped down to ~2e-7 Torr. HS cooling water valves were opened, no leaks detected.
TGHT was stepped up to 35A, voltage max set at 13V. TBHT currently @ 0A.
Waited ~20min, current stabilized, vacuum started to drop, auto-ramp initiated at 2.0A/min and max setpoint to 700A.
Good vacuum: 3.00e-5 Torr, Bad vacuum 4.00e-5 Torr.
|
Tuesday, January 21, 2014, 11:51
Vacuum was grumpy and was well on it's way to tripping off [reached 5e-5 Torr], auto ramping was stopped at ~95A and quickly stepped down to 90A to avoid tripping it off.
Allowed vacuum to settle back down to 2.3e-6 Torr. Auto ramping changed to 0.2A/min and re-started.
close-call!
|
Wednesday, January 22, 2014, 09:46
TGHT has been slowly ramping up overnight at a rate of 0.2A/min.
IGP1 = 2.9e-7 Torr, TGHT = 342A; stepping ramping rate up to 2.0A/min.
|
Wednesday, January 22, 2014, 13:43
TGHT is sitting at 693A, IGP1 = 1.3e-6 Torr.
Stepping up TGHT voltage up to 14V from 13.05V to reach the max current of 700A.
|
Wednesday, January 22, 2014, 15:09
TGHT reached to 700A/12.83V. Local temperature on the boat surface was measured at ~1500C.
Note: This is the "old" design boat. The new design boat was able to heat up to 900A/16.88 - the temperature was measured at about 1500C. (see elog: https://elog.triumf.ca/TIS/Evaporator_2/15)
Target will be heated for a few hours and will be cooled down later tonight.
The chamber will be vented tomorrow and the boat will be inspected.
|
Wednesday, January 22, 2014, 18:22, John Wong, Empty, 40282-4, TARGET BOAT, Problems, Sintering Ta target boat with TaC coating (IEVAP2:TBHT2 water signal problem)
|
John Wong wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Monday, January 20, 2014, 16:32
A new target boat was sprayed with TaC coating and let dry this morning.
The target boat is NOT wrapped with Ta-heat shield.
The boat was installed in Evap#2, chamber is currently being pumped down overnight.
|
Tuesday, January 21, 2014, 11:10
Chamber was pumped down to ~2e-7 Torr. HS cooling water valves were opened, no leaks detected.
TGHT was stepped up to 35A, voltage max set at 13V. TBHT currently @ 0A.
Waited ~20min, current stabilized, vacuum started to drop, auto-ramp initiated at 2.0A/min and max setpoint to 700A.
Good vacuum: 3.00e-5 Torr, Bad vacuum 4.00e-5 Torr.
|
Tuesday, January 21, 2014, 11:51
Vacuum was grumpy and was well on it's way to tripping off [reached 5e-5 Torr], auto ramping was stopped at ~95A and quickly stepped down to 90A to avoid tripping it off.
Allowed vacuum to settle back down to 2.3e-6 Torr. Auto ramping changed to 0.2A/min and re-started.
close-call!
|
Wednesday, January 22, 2014, 09:46
TGHT has been slowly ramping up overnight at a rate of 0.2A/min.
IGP1 = 2.9e-7 Torr, TGHT = 342A; stepping ramping rate up to 2.0A/min.
|
Wednesday, January 22, 2014, 13:43
TGHT is sitting at 693A, IGP1 = 1.3e-6 Torr.
Stepping up TGHT voltage up to 14V from 13.05V to reach the max current of 700A.
|
Wednesday, January 22, 2014, 15:09
TGHT reached to 700A/12.83V. Local temperature on the boat surface was measured at ~1500C.
Target will be heated for a few hours and will be cooled down later tonight.
The chamber will be vented tomorrow and the boat will be inspected.
|
Wednesday, January 22, 2014, 18:09
After the boat was heated for ~4hrs, TGHT tripped off on IEVAP2:TBHT2 (see attachment #1, #2).
Tried clearing the water interlock via EPICS - failed to clear. Checked the local water valves - ALL VALVES are OPEN
Tried closing and re-opening the IEVAP2:TBHT2 valves, interlock cleared after a few minutes.
Maybe a fault in the water signal. If it happens again, the water signal should be replaced.
Turned back on the power supply - TGHT current/voltage are holding. Target boat may be OK!
Chamber is a bit warm now. Will allow time to cool down.
Will vent the chamber tomorrow and the boat will be inspected.
|
Thursday, January 23, 2014, 16:22, Laura Lambert, Empty, 40282-4, TARGET BOAT, Problems resolved, Sintering Ta target boat with TaC coating
|
John Wong wrote: |
John Wong wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Monday, January 20, 2014, 16:32
A new target boat was sprayed with TaC coating and let dry this morning.
The target boat is NOT wrapped with Ta-heat shield.
The boat was installed in Evap#2, chamber is currently being pumped down overnight.
|
Tuesday, January 21, 2014, 11:10
Chamber was pumped down to ~2e-7 Torr. HS cooling water valves were opened, no leaks detected.
TGHT was stepped up to 35A, voltage max set at 13V. TBHT currently @ 0A.
Waited ~20min, current stabilized, vacuum started to drop, auto-ramp initiated at 2.0A/min and max setpoint to 700A.
Good vacuum: 3.00e-5 Torr, Bad vacuum 4.00e-5 Torr.
|
Tuesday, January 21, 2014, 11:51
Vacuum was grumpy and was well on it's way to tripping off [reached 5e-5 Torr], auto ramping was stopped at ~95A and quickly stepped down to 90A to avoid tripping it off.
Allowed vacuum to settle back down to 2.3e-6 Torr. Auto ramping changed to 0.2A/min and re-started.
close-call!
|
Wednesday, January 22, 2014, 09:46
TGHT has been slowly ramping up overnight at a rate of 0.2A/min.
IGP1 = 2.9e-7 Torr, TGHT = 342A; stepping ramping rate up to 2.0A/min.
|
Wednesday, January 22, 2014, 13:43
TGHT is sitting at 693A, IGP1 = 1.3e-6 Torr.
Stepping up TGHT voltage up to 14V from 13.05V to reach the max current of 700A.
|
Wednesday, January 22, 2014, 15:09
TGHT reached to 700A/12.83V. Local temperature on the boat surface was measured at ~1500C.
Target will be heated for a few hours and will be cooled down later tonight.
The chamber will be vented tomorrow and the boat will be inspected.
|
Wednesday, January 22, 2014, 18:09
After the boat was heated for ~4hrs, TGHT tripped off on IEVAP2:TBHT2 (see attachment #1, #2).
Tried clearing the water interlock via EPICS - failed to clear. Checked the local water valves - ALL VALVES are OPEN
Tried closing and re-opening the IEVAP2:TBHT2 valves, interlock cleared after a few minutes.
Maybe a fault in the water signal. If it happens again, the water signal should be replaced.
Turned back on the power supply - TGHT current/voltage are holding. Target boat may be OK!
Chamber is a bit warm now. Will allow time to cool down.
Will vent the chamber tomorrow and the boat will be inspected.
|
Thursday, January 23, 2014, 16:18
Chamber vented overnight and was opened up this morning.
Target boat not fully sintered [see attached photos].
Chamber currently being pumped down again in order to continue with sintering TaC coating.
HS cooling water valves were opened, no leaks detected.
Will ramp up to 700A again over the weekend. |
Friday, January 24, 2014, 14:25, Laura Lambert, Empty, 40282-4, TARGET BOAT, In progress, Sintering Ta target boat with TaC coating
|
Laura Lambert wrote: |
John Wong wrote: |
John Wong wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Monday, January 20, 2014, 16:32
A new target boat was sprayed with TaC coating and let dry this morning.
The target boat is NOT wrapped with Ta-heat shield.
The boat was installed in Evap#2, chamber is currently being pumped down overnight.
|
Tuesday, January 21, 2014, 11:10
Chamber was pumped down to ~2e-7 Torr. HS cooling water valves were opened, no leaks detected.
TGHT was stepped up to 35A, voltage max set at 13V. TBHT currently @ 0A.
Waited ~20min, current stabilized, vacuum started to drop, auto-ramp initiated at 2.0A/min and max setpoint to 700A.
Good vacuum: 3.00e-5 Torr, Bad vacuum 4.00e-5 Torr.
|
Tuesday, January 21, 2014, 11:51
Vacuum was grumpy and was well on it's way to tripping off [reached 5e-5 Torr], auto ramping was stopped at ~95A and quickly stepped down to 90A to avoid tripping it off.
Allowed vacuum to settle back down to 2.3e-6 Torr. Auto ramping changed to 0.2A/min and re-started.
close-call!
|
Wednesday, January 22, 2014, 09:46
TGHT has been slowly ramping up overnight at a rate of 0.2A/min.
IGP1 = 2.9e-7 Torr, TGHT = 342A; stepping ramping rate up to 2.0A/min.
|
Wednesday, January 22, 2014, 13:43
TGHT is sitting at 693A, IGP1 = 1.3e-6 Torr.
Stepping up TGHT voltage up to 14V from 13.05V to reach the max current of 700A.
|
Wednesday, January 22, 2014, 15:09
TGHT reached to 700A/12.83V. Local temperature on the boat surface was measured at ~1500C.
Target will be heated for a few hours and will be cooled down later tonight.
The chamber will be vented tomorrow and the boat will be inspected.
|
Wednesday, January 22, 2014, 18:09
After the boat was heated for ~4hrs, TGHT tripped off on IEVAP2:TBHT2 (see attachment #1, #2).
Tried clearing the water interlock via EPICS - failed to clear. Checked the local water valves - ALL VALVES are OPEN
Tried closing and re-opening the IEVAP2:TBHT2 valves, interlock cleared after a few minutes.
Maybe a fault in the water signal. If it happens again, the water signal should be replaced.
Turned back on the power supply - TGHT current/voltage are holding. Target boat may be OK!
Chamber is a bit warm now. Will allow time to cool down.
Will vent the chamber tomorrow and the boat will be inspected.
|
Thursday, January 23, 2014, 16:18
Chamber vented overnight and was opened up this morning.
Target boat not fully sintered [see attached photos].
Chamber currently being pumped down again in order to continue with sintering TaC coating.
HS cooling water valves were opened, no leaks detected.
Will ramp up to 700A again over the weekend.
|
Friday, January 24, 2014, 14:21
Chamber was pumped down to 1.7e-7 Torr.
TGHT was stepped up to 35A, voltage max set at 14V. TBHT currently sitting at 0A.
Waited 20min, vacuum consistently stable. Auto-ramp initiated at 2.0 A/min and max setpoint to 700A.
|
Monday, January 27, 2014, 10:59, Laura Lambert, Empty, 40282-4, TARGET BOAT, In progress, Sintering Ta target boat with TaC coating
|
Laura Lambert wrote: |
Laura Lambert wrote: |
John Wong wrote: |
John Wong wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Monday, January 20, 2014, 16:32
A new target boat was sprayed with TaC coating and let dry this morning.
The target boat is NOT wrapped with Ta-heat shield.
The boat was installed in Evap#2, chamber is currently being pumped down overnight.
|
Tuesday, January 21, 2014, 11:10
Chamber was pumped down to ~2e-7 Torr. HS cooling water valves were opened, no leaks detected.
TGHT was stepped up to 35A, voltage max set at 13V. TBHT currently @ 0A.
Waited ~20min, current stabilized, vacuum started to drop, auto-ramp initiated at 2.0A/min and max setpoint to 700A.
Good vacuum: 3.00e-5 Torr, Bad vacuum 4.00e-5 Torr.
|
Tuesday, January 21, 2014, 11:51
Vacuum was grumpy and was well on it's way to tripping off [reached 5e-5 Torr], auto ramping was stopped at ~95A and quickly stepped down to 90A to avoid tripping it off.
Allowed vacuum to settle back down to 2.3e-6 Torr. Auto ramping changed to 0.2A/min and re-started.
close-call!
|
Wednesday, January 22, 2014, 09:46
TGHT has been slowly ramping up overnight at a rate of 0.2A/min.
IGP1 = 2.9e-7 Torr, TGHT = 342A; stepping ramping rate up to 2.0A/min.
|
Wednesday, January 22, 2014, 13:43
TGHT is sitting at 693A, IGP1 = 1.3e-6 Torr.
Stepping up TGHT voltage up to 14V from 13.05V to reach the max current of 700A.
|
Wednesday, January 22, 2014, 15:09
TGHT reached to 700A/12.83V. Local temperature on the boat surface was measured at ~1500C.
Target will be heated for a few hours and will be cooled down later tonight.
The chamber will be vented tomorrow and the boat will be inspected.
|
Wednesday, January 22, 2014, 18:09
After the boat was heated for ~4hrs, TGHT tripped off on IEVAP2:TBHT2 (see attachment #1, #2).
Tried clearing the water interlock via EPICS - failed to clear. Checked the local water valves - ALL VALVES are OPEN
Tried closing and re-opening the IEVAP2:TBHT2 valves, interlock cleared after a few minutes.
Maybe a fault in the water signal. If it happens again, the water signal should be replaced.
Turned back on the power supply - TGHT current/voltage are holding. Target boat may be OK!
Chamber is a bit warm now. Will allow time to cool down.
Will vent the chamber tomorrow and the boat will be inspected.
|
Thursday, January 23, 2014, 16:18
Chamber vented overnight and was opened up this morning.
Target boat not fully sintered [see attached photos].
Chamber currently being pumped down again in order to continue with sintering TaC coating.
HS cooling water valves were opened, no leaks detected.
Will ramp up to 700A again over the weekend.
|
Friday, January 24, 2014, 14:21
Chamber was pumped down to 1.7e-7 Torr.
TGHT was stepped up to 35A, voltage max set at 14V. TBHT currently sitting at 0A.
Waited 20min, vacuum consistently stable. Auto-ramp initiated at 2.0 A/min and max setpoint to 700A.
|
Monday, January 27, 2014, 10:05
TGHT reached 700A over the weekend. Measured temp @ 2000C.
TGHT auto-cool inititated at 2.0A/min.
|
Tuesday, January 28, 2014, 11:57, Laura Lambert, Empty, 40282-4, TARGET BOAT, In progress, Sintering Ta target boat with TaC coating
|
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
John Wong wrote: |
John Wong wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Monday, January 20, 2014, 16:32
A new target boat was sprayed with TaC coating and let dry this morning.
The target boat is NOT wrapped with Ta-heat shield.
The boat was installed in Evap#2, chamber is currently being pumped down overnight.
|
Tuesday, January 21, 2014, 11:10
Chamber was pumped down to ~2e-7 Torr. HS cooling water valves were opened, no leaks detected.
TGHT was stepped up to 35A, voltage max set at 13V. TBHT currently @ 0A.
Waited ~20min, current stabilized, vacuum started to drop, auto-ramp initiated at 2.0A/min and max setpoint to 700A.
Good vacuum: 3.00e-5 Torr, Bad vacuum 4.00e-5 Torr.
|
Tuesday, January 21, 2014, 11:51
Vacuum was grumpy and was well on it's way to tripping off [reached 5e-5 Torr], auto ramping was stopped at ~95A and quickly stepped down to 90A to avoid tripping it off.
Allowed vacuum to settle back down to 2.3e-6 Torr. Auto ramping changed to 0.2A/min and re-started.
close-call!
|
Wednesday, January 22, 2014, 09:46
TGHT has been slowly ramping up overnight at a rate of 0.2A/min.
IGP1 = 2.9e-7 Torr, TGHT = 342A; stepping ramping rate up to 2.0A/min.
|
Wednesday, January 22, 2014, 13:43
TGHT is sitting at 693A, IGP1 = 1.3e-6 Torr.
Stepping up TGHT voltage up to 14V from 13.05V to reach the max current of 700A.
|
Wednesday, January 22, 2014, 15:09
TGHT reached to 700A/12.83V. Local temperature on the boat surface was measured at ~1500C.
Target will be heated for a few hours and will be cooled down later tonight.
The chamber will be vented tomorrow and the boat will be inspected.
|
Wednesday, January 22, 2014, 18:09
After the boat was heated for ~4hrs, TGHT tripped off on IEVAP2:TBHT2 (see attachment #1, #2).
Tried clearing the water interlock via EPICS - failed to clear. Checked the local water valves - ALL VALVES are OPEN
Tried closing and re-opening the IEVAP2:TBHT2 valves, interlock cleared after a few minutes.
Maybe a fault in the water signal. If it happens again, the water signal should be replaced.
Turned back on the power supply - TGHT current/voltage are holding. Target boat may be OK!
Chamber is a bit warm now. Will allow time to cool down.
Will vent the chamber tomorrow and the boat will be inspected.
|
Thursday, January 23, 2014, 16:18
Chamber vented overnight and was opened up this morning.
Target boat not fully sintered [see attached photos].
Chamber currently being pumped down again in order to continue with sintering TaC coating.
HS cooling water valves were opened, no leaks detected.
Will ramp up to 700A again over the weekend.
|
Friday, January 24, 2014, 14:21
Chamber was pumped down to 1.7e-7 Torr.
TGHT was stepped up to 35A, voltage max set at 14V. TBHT currently sitting at 0A.
Waited 20min, vacuum consistently stable. Auto-ramp initiated at 2.0 A/min and max setpoint to 700A.
|
Monday, January 27, 2014, 10:05
TGHT reached 700A over the weekend. Measured temp @ 2000C.
TGHT auto-cool inititated at 2.0A/min.
|
Tuesday, January 28, 2014, 11:53
Chamber cooled down overnight, vented and opened up this morning.
Target boat still has a strip of green, still not fully sintered! [see attached photos].
Chamber currently being pumped down again to attempt sintering - round 3.
|
Tuesday, January 28, 2014, 13:09, Laura Lambert, Empty, 40282-4, TARGET BOAT, Done, Sintering Ta target boat with TaC coating
|
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
John Wong wrote: |
John Wong wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Laura Lambert wrote: |
Monday, January 20, 2014, 16:32
A new target boat was sprayed with TaC coating and let dry this morning.
The target boat is NOT wrapped with Ta-heat shield.
The boat was installed in Evap#2, chamber is currently being pumped down overnight.
|
Tuesday, January 21, 2014, 11:10
Chamber was pumped down to ~2e-7 Torr. HS cooling water valves were opened, no leaks detected.
TGHT was stepped up to 35A, voltage max set at 13V. TBHT currently @ 0A.
Waited ~20min, current stabilized, vacuum started to drop, auto-ramp initiated at 2.0A/min and max setpoint to 700A.
Good vacuum: 3.00e-5 Torr, Bad vacuum 4.00e-5 Torr.
|
Tuesday, January 21, 2014, 11:51
Vacuum was grumpy and was well on it's way to tripping off [reached 5e-5 Torr], auto ramping was stopped at ~95A and quickly stepped down to 90A to avoid tripping it off.
Allowed vacuum to settle back down to 2.3e-6 Torr. Auto ramping changed to 0.2A/min and re-started.
close-call!
|
Wednesday, January 22, 2014, 09:46
TGHT has been slowly ramping up overnight at a rate of 0.2A/min.
IGP1 = 2.9e-7 Torr, TGHT = 342A; stepping ramping rate up to 2.0A/min.
|
Wednesday, January 22, 2014, 13:43
TGHT is sitting at 693A, IGP1 = 1.3e-6 Torr.
Stepping up TGHT voltage up to 14V from 13.05V to reach the max current of 700A.
|
Wednesday, January 22, 2014, 15:09
TGHT reached to 700A/12.83V. Local temperature on the boat surface was measured at ~1500C.
Target will be heated for a few hours and will be cooled down later tonight.
The chamber will be vented tomorrow and the boat will be inspected.
|
Wednesday, January 22, 2014, 18:09
After the boat was heated for ~4hrs, TGHT tripped off on IEVAP2:TBHT2 (see attachment #1, #2).
Tried clearing the water interlock via EPICS - failed to clear. Checked the local water valves - ALL VALVES are OPEN
Tried closing and re-opening the IEVAP2:TBHT2 valves, interlock cleared after a few minutes.
Maybe a fault in the water signal. If it happens again, the water signal should be replaced.
Turned back on the power supply - TGHT current/voltage are holding. Target boat may be OK!
Chamber is a bit warm now. Will allow time to cool down.
Will vent the chamber tomorrow and the boat will be inspected.
|
Thursday, January 23, 2014, 16:18
Chamber vented overnight and was opened up this morning.
Target boat not fully sintered [see attached photos].
Chamber currently being pumped down again in order to continue with sintering TaC coating.
HS cooling water valves were opened, no leaks detected.
Will ramp up to 700A again over the weekend.
|
Friday, January 24, 2014, 14:21
Chamber was pumped down to 1.7e-7 Torr.
TGHT was stepped up to 35A, voltage max set at 14V. TBHT currently sitting at 0A.
Waited 20min, vacuum consistently stable. Auto-ramp initiated at 2.0 A/min and max setpoint to 700A.
|
Monday, January 27, 2014, 10:05
TGHT reached 700A over the weekend. Measured temp @ 2000C.
TGHT auto-cool inititated at 2.0A/min.
|
Tuesday, January 28, 2014, 11:53
Chamber cooled down overnight, vented and opened up this morning.
Target boat still has a strip of green, still not fully sintered! [see attached photos].
Chamber currently being pumped down again to attempt sintering - round 3.
|
Tuesday, January 28, 2014, 13:06
Discussed with Peter. Instead of re-sintering the whole boat by itself, end caps will be inserted for sintering and will be placed further down the boat where the sintering process appears complete.
|
Wednesday, January 15, 2014, 17:45, John Wong, Empty, 39165-9, LP-SIS, In progress, Sintering TaC coating container
|
Wednesday, January 15, 2014, 17:30
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min.
TBHT will be ramped up to 230A at 0.2A/min.
Chamber is currently being pumped. Tomorrow, the HS water valve can be opened to test for leaks.
Notes:
If everything is fine, TGHT/TBHT can be stepped up to 30A-50A. Watch for the vacuum; once it's stable the auto ramping program can be initiated.
Once TGHT/TBHT reached above 200A, the ramping rate for TGHT can be increased up to 2A/min. (This step is to speed up the process; however it's not mandatory)
|
Thursday, January 16, 2014, 13:06, Laura Lambert, Empty, 39165-9, LP-SIS, In progress, Sintering TaC coating container
|
John Wong wrote: |
Wednesday, January 15, 2014, 17:30
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min.
TBHT will be ramped up to 230A at 0.2A/min.
Chamber is currently being pumped. Tomorrow, the HS water valve can be opened to test for leaks.
Notes:
If everything is fine, TGHT/TBHT can be stepped up to 30A-50A. Watch for the vacuum; once it's stable the auto ramping program can be initiated.
Once TGHT/TBHT reached above 200A, the ramping rate for TGHT can be increased up to 2A/min. (This step is to speed up the process; however it's not mandatory)
|
Thursday, January 16, 2014, 11:35
Chamber was pumped down overnight to 10-7 Torr. HS water valve was opened and no leak in vacuum was observed.
TGHT and TBHT were stepped up to 35A. Waited ~30min, current stabilized and vacuum starting to drop.
Initiating auto-ramping: Good Vac = 2.0e-5 Torr, Bad Vac = 3.0e-5 Torr.
|
Friday, January 17, 2014, 09:34, John Wong, Empty, 39165-9, LP-SIS, In progress, Sintering TaC coating container
|
Laura Lambert wrote: |
John Wong wrote: |
Wednesday, January 15, 2014, 17:30
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min.
TBHT will be ramped up to 230A at 0.2A/min.
Chamber is currently being pumped. Tomorrow, the HS water valve can be opened to test for leaks.
Notes:
If everything is fine, TGHT/TBHT can be stepped up to 30A-50A. Watch for the vacuum; once it's stable the auto ramping program can be initiated.
Once TGHT/TBHT reached above 200A, the ramping rate for TGHT can be increased up to 2A/min. (This step is to speed up the process; however it's not mandatory)
|
Thursday, January 16, 2014, 11:35
Chamber was pumped down overnight to 10-7 Torr. HS water valve was opened and no leak in vacuum was observed.
TGHT and TBHT were stepped up to 35A. Waited ~30min, current stabilized and vacuum starting to drop.
Initiating auto-ramping: Good Vac = 2.0e-5 Torr, Bad Vac = 3.0e-5 Torr.
|
Friday, January 17, 2014, 09:28
TGHT/TBHT @ 300/200A. TBHT voltage is limited at 3A.
TGHT ramping rate increased to 2A/min. Pressure @ 4.5e-7 Torr.
|
Friday, January 17, 2014, 10:18, Laura Lambert, Empty, 39165-9, LP-SIS, In progress, Sintering TaC coating container
|
John Wong wrote: |
Laura Lambert wrote: |
John Wong wrote: |
Wednesday, January 15, 2014, 17:30
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min.
TBHT will be ramped up to 230A at 0.2A/min.
Chamber is currently being pumped. Tomorrow, the HS water valve can be opened to test for leaks.
Notes:
If everything is fine, TGHT/TBHT can be stepped up to 30A-50A. Watch for the vacuum; once it's stable the auto ramping program can be initiated.
Once TGHT/TBHT reached above 200A, the ramping rate for TGHT can be increased up to 2A/min. (This step is to speed up the process; however it's not mandatory)
|
Thursday, January 16, 2014, 11:35
Chamber was pumped down overnight to 10-7 Torr. HS water valve was opened and no leak in vacuum was observed.
TGHT and TBHT were stepped up to 35A. Waited ~30min, current stabilized and vacuum starting to drop.
Initiating auto-ramping: Good Vac = 2.0e-5 Torr, Bad Vac = 3.0e-5 Torr.
|
Friday, January 17, 2014, 09:28
TGHT/TBHT @ 300/200A. TBHT voltage is limited at 3A.
TGHT ramping rate increased to 2A/min. Pressure @ 4.5e-7 Torr.
|
Friday, January 17, 2014, 10:14
TBHT stopped at 200A with voltage limit sitting at 3V.
Aborted auto-ramp, changed the voltage limit to 5V and increased ramping rate to 2A/min. Re-started auto-ramp.
IGP1 @ 5.0e-7 Torr
|
Friday, January 17, 2014, 12:52, John Wong, Empty, 39165-9, LP-SIS, In progress, Sintering TaC coating container
|
Laura Lambert wrote: |
John Wong wrote: |
Laura Lambert wrote: |
John Wong wrote: |
Wednesday, January 15, 2014, 17:30
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min.
TBHT will be ramped up to 230A at 0.2A/min.
Chamber is currently being pumped. Tomorrow, the HS water valve can be opened to test for leaks.
Notes:
If everything is fine, TGHT/TBHT can be stepped up to 30A-50A. Watch for the vacuum; once it's stable the auto ramping program can be initiated.
Once TGHT/TBHT reached above 200A, the ramping rate for TGHT can be increased up to 2A/min. (This step is to speed up the process; however it's not mandatory)
|
Thursday, January 16, 2014, 11:35
Chamber was pumped down overnight to 10-7 Torr. HS water valve was opened and no leak in vacuum was observed.
TGHT and TBHT were stepped up to 35A. Waited ~30min, current stabilized and vacuum starting to drop.
Initiating auto-ramping: Good Vac = 2.0e-5 Torr, Bad Vac = 3.0e-5 Torr.
|
Friday, January 17, 2014, 09:28
TGHT/TBHT @ 300/200A. TBHT voltage is limited at 3A.
TGHT ramping rate increased to 2A/min. Pressure @ 4.5e-7 Torr.
|
Friday, January 17, 2014, 10:14
TBHT stopped at 200A with voltage limit sitting at 3V.
Aborted auto-ramp, changed the voltage limit to 5V and increased ramping rate to 2A/min. Re-started auto-ramp.
IGP1 @ 5.0e-7 Torr
|
Friday, January 17, 2014, 12:45
TGHT voltage limiting at 9.9V, and current stayed at 560A. Increased the TGHT voltage to 10.5V and continued ramping the heater up.
TGHT/TBHT stabilized at 580A (~10V) and 230A(3.6V).
Pressure at 1.03e-6 Torr and coming down...
Target will be heated until 5pm (4hrs) before cooling down at the ramping rate of 2A/min.
Chamber will be vented in air, next week.
Friday, January 17, 2014, 16:51
Auto-cooling initiated at 2A/min.
Vac @ 5.3e-7 Torr.
|
Monday, January 20, 2014, 16:30, Laura Lambert, Empty, 39165-9, LP-SIS, Done, Sintering TaC coating container
|
John Wong wrote: |
Laura Lambert wrote: |
John Wong wrote: |
Laura Lambert wrote: |
John Wong wrote: |
Wednesday, January 15, 2014, 17:30
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min.
TBHT will be ramped up to 230A at 0.2A/min.
Chamber is currently being pumped. Tomorrow, the HS water valve can be opened to test for leaks.
Notes:
If everything is fine, TGHT/TBHT can be stepped up to 30A-50A. Watch for the vacuum; once it's stable the auto ramping program can be initiated.
Once TGHT/TBHT reached above 200A, the ramping rate for TGHT can be increased up to 2A/min. (This step is to speed up the process; however it's not mandatory)
|
Thursday, January 16, 2014, 11:35
Chamber was pumped down overnight to 10-7 Torr. HS water valve was opened and no leak in vacuum was observed.
TGHT and TBHT were stepped up to 35A. Waited ~30min, current stabilized and vacuum starting to drop.
Initiating auto-ramping: Good Vac = 2.0e-5 Torr, Bad Vac = 3.0e-5 Torr.
|
Friday, January 17, 2014, 09:28
TGHT/TBHT @ 300/200A. TBHT voltage is limited at 3A.
TGHT ramping rate increased to 2A/min. Pressure @ 4.5e-7 Torr.
|
Friday, January 17, 2014, 10:14
TBHT stopped at 200A with voltage limit sitting at 3V.
Aborted auto-ramp, changed the voltage limit to 5V and increased ramping rate to 2A/min. Re-started auto-ramp.
IGP1 @ 5.0e-7 Torr
|
Friday, January 17, 2014, 12:45
TGHT voltage limiting at 9.9V, and current stayed at 560A. Increased the TGHT voltage to 10.5V and continued ramping the heater up.
TGHT/TBHT stabilized at 850A (~10V) and 230A(3.6V).
Pressure at 1.03e-6 Torr and coming down...
Target will be heated until 5pm (4hrs) before cooling down at the ramping rate of 2A/min.
Chamber will be vented in air, next week.
Friday, January 17, 2014, 16:51
Auto-cooling initiated at 2A/min.
Vac @ 5.3e-7 Torr.
|
|
Thursday, November 07, 2013, 09:38, Anders Mjos, , , , Problems resolved, Heat Shield cooling line twisted
|
See attached photo.
The Heat Shield has been taken to the Machine Shop for repair.
Friday, November 08, 2013
The Heat Shield cooling line has been repaired and the lid re-installed in the evaporator. Photo attached.
Friday, November 08, 2013, 10:58 : Roughing Started
Friday, November 08, 2013, 11:05: Turbo started
Friday, November 08, 2013, 11:15: Turbo at speed Vacuum at (IGP1) 5.7E-5 T |
Wednesday, November 06, 2013, 17:36, John Wong, TaC, Target Boat #2, , In progress, Testing TaC matrix coating
|
The purpose of this experiment is to improve the TaC coating mixed with other metals as additives. The coating solution will be sprayed on Ta metal (0.015" thick, same thickness as the target container).
The samples will be sintered at ~ 1800C. Once the process is completed, a graphite tube will be inserted into the tube, and then re-heated it up to 1800C.
This test will show how good the protective layer to prevent the graphite to react with the Ta metal.
Wednesday, November 06, 2013, 17:11
Step #1
Two samples:
1. A short tube (same diameter as the usual container)
2. A cross section of the tube.
Both samples are coated with the TaC matrix spray:
0.05 moles TaC
0.005 moles of Mo2C, VC, Cr3C2, NbC
A Rh foil is used as a protective under layer.
see links for pictures: https://www.dropbox.com/sh/866zsp44nnjeg2z/LqCThu-G_0
The target boat is wrapped with 3 layers of heat shields.
Samples will be heated up to 600A ~1800C
Chamber is currently being pumped down.
Friday, November 08, 2013, 17:13
Chamber was pumped down to ~2e-6 Torr. HS water valve is opened and no leaks were detected.
TGHT will be ramped up to 580A at 1A/min.
Monday, November 11, 2013, 08:10
TGHT has reached to 580A; samples has been heated at that current for over the weekend.
IGP2 currently at 3.5e-7 Torr.
Auto cooling initiated, ramping rate at -2.0A/min.
Step 2:
The coated tube is sintered with TaC-matrix.
The graphite tube is inserted in the tube and will be heated back up; see link for details:
https://www.dropbox.com/sh/ji0rhlj0v1tfj1w/cRv1I3VJXE
Chamber is currently pumped down to 1.8e-6 Torr.
TGHT will first be ramped up to 450A (1A/min) to see how the reaction behaves, then a caution ramp up to 600A will take place.
Friday, November 15, 2013, 11:04
TGHT reached to 450A. Cooling down to 0A. Chamber will be vented for inspection.
Monday, November 18, 2013, 17:22
Continue Step#2:
The sample looks ok after heating at 450A.
Re-heating it to 500A.
Chamber has been pumped down to 4.0e-6 Torr.
Initiated auto-ramping...
|
Friday, November 01, 2013, 17:20, Anders Mjos, , , , Problems, Backing pump needs new filter
|
The source of the poor vacuum in the backing line seems to be related to a dirty filter. We will try to find a replacement filter next week.
The problem seem to have started September 17th, when backing preassure CG1A went from 40 mTorr to 130 mTorr. CG1B remained around 30 mTorr. |
Monday, November 04, 2013, 14:02, Anders Mjos, , , , Maintenance, Backing pump replaced
|
Anders Mjos wrote: |
The source of the poor vacuum in the backing line seems to be related to a dirty filter. We will try to find a replacement filter next week.
The problem seem to have started September 17th, when backing preassure CG1A went from 40 mTorr to 130 mTorr. CG1B remained around 30 mTorr.
|
With the help of Anthony Ip from vacuum group, the problem was diagnosed to be the roughing pump itself. The pump was replaced and pumping improved. The chamber can now be evacuated and turbo ready to start in less than 10 minutes.
The filter is not stocked by vacuum group and could not be replaced.
Last week parts of the roughing line was cleaned by Rick. The PVC roughing line has been replaced with a SST bellows. The SST bellows is KF25 and should be replaced by a KF40 bellows in the long run. |
Tuesday, October 29, 2013, 15:50, Anders Mjos, , , , In progress, Copper bars on TGHT and TBHT
|
Tuesday, October 29, 2013, 15:50: Pumping down
Wednesday, October 30, 2013, 09:32: Turbo started
Wednesday, October 30, 2013, 14:50: The Cu-bars were heated to 600A and 300A for TGHT and TBHT respectively.
Wednesday, October 30, 2013, 15:17: PS off. Turbo off.
Results can be found on DocuShare and in the attached plot. |
Friday, October 04, 2013, 16:21, John Wong, Empty, , LP-SIS, Done, Sintering TaC coating on a LP target container to be used for C-grv tube test
|
Friday, October 04, 2013, 15:37
A LP target container is coated with TaC. The container is wrapped with 3 layers to heat shield.
This container will be used for the graphite tube test.
Chamber is being pumped down.
The HS cooling water valves are open and no leaks are detected.
TGHT will be ramped up to 580A at 0.2A/min
TBHT will be ramped up to 230A at 0.2A/min.
The temperature will be monitored and measured.
Sunday, October 06, 2013, 19:55
TGHT and TBHT have reached to 580A/230A, respectively. And the target has been heated for about 5 hours.
The temperature inside the tube is measure at 1000C; this is much lower than expected as to previously measured at 1700C.
The temperature outside the container is at 1400C.
I'm suspecting the thermocouple inside the tube could be shorted.
Cooling down the heaters down to zero at 2A/min for TGHT and 1A/min for TBHT.
Tomorrow, the chamber will be vented and the target will be inspected.
I like to re-adjust the thermocouple again, and re-heat the target back up, hoping to reach 1700C at TGHT = 580A.
Monday, October 07, 2013, 15:24
The sintering of the TaC coating is complete.
The chamber was vented this morning. Apparently, there was a short in the thermocouple so the temperature measure was recorded much lower.
The thermocouples are adjusted, and the chamber is pumped down.
Vac currently at 1.17e-6 Torr.
TGHT and TBHT will be ramped up to 580A/230A at 2A/min.
Continue monitoring the temperature...
Monday, October 07, 2013, 16:13
TGHT and TBHT were ramped up to 90A. Temperature inside the tube was measure just at 75C and the outside surface was at 207C.
Maybe the thermocouple is F up; will replace with a new one tomorrow.
Cooling down the target down...
Tuesday, October 22, 2013, 16:49
The target was heated up to 580A and the temperature inside the tube was measured to be ~1800C and the outside surface was ~1400C.
The target was cooled down. Then the graphite tube was inserted.
There are two thermcouples inserted inside the tube on both ends.
Chamber has been pumped down to 4.33 e-7 Torr. No leaks were detected.
Target will be heated up again to TGHT @ 580A / TBHT @ 230A at 0.2A/min.
The temperatures will be monitored.
T1 = left (floating)
T2 = right (toughing C-grv tube)
(wtf ionizer pointing into the page).
Thursday, October 24, 2013, 16:35
TGHT/TBHT reached to 580A/230A.
T1 = 1642C
T2 = Error?? Reading goes on/off intermittently, showing 900 - 1900C
Thursday, October 24, 2013, 16:45
Ramping up TGHT to 680A to see if T1 can reach 1700C.
IG1 currently at 5.2e-7 Torr.
Friday, October 25, 2013, 12:30
TGHT was ramped up to 632A (stopped due to voltage limiting).
T1 was measured at 1960C. Vac went up as it was heated up. (see attachment #2)
Target was cooled down at 5A/min, now at 0A.
The chamber will be vented and the target will be inspected.
This run is complete.
|
Thursday, September 26, 2013, 15:17, John Wong, Empty, 39814-VI-?, LP-IG-LIS, Done, Sintering empty target oven coated with TaC for UCx#8
|
Thursday, September 26, 2013, 13:04
The LP-IG-LIS target container is coated with TaC.
Container is wrapped with 3 layers of Ta heat shield and about to go through the sintering process.
A thermocouple is inserted to measure the temperature inside the tube (1st attempt ever).
Click on the link for detailed pictures:
https://www.dropbox.com/sh/6dc5arajg87mws9/6cU5OxjkZg
TGHT will be ramped up to 580A at 0.2A/min
TBHT will be ramped up to 230A at 0.2A/min.
Chamber has been pumped down. HS cooling H2O valves are opened, and no leaks are detected.
Currently IGP1 @ 5.9e-6 Torr.
Thursday, September 26, 2013, 15:44
TGHT stepped up to 30A. TBHT currently @ 0A.
Temp @ 35C, Vac @ 1.4e-5 Torr.
Monday, September 30, 2013, 14:54
The container was heated up to 580A TGHT/ 230A TBHT for a day (see attachment #1 for vac vs cur plot).
The temperature was measure at ~1780C. (see link for details: https://www.dropbox.com/sh/d8d9j2t60qlm3jk/nkMh7dx_R8 )
The target was cooled down and vented.
Proceed complete.
|
Tuesday, September 17, 2013, 11:21, John Wong, Nb, target boat #3 (brand new!) , , , Nb thermo treatment (Bob's samples)
|
Tuesday, September 17, 2013, 11:14
Target boat contains 5 Nb discs. 3 discs are wraps with 0.001" thin of Nb foil (99.8% pure), and 2 are wraps with 0.001" Ta foil (see attachment#1)
Chamber has been pumped down over night. Pressure is currently at 9.8e-7 Torr.
Heating instructions:
Samples will be heated up to 800C. TGHT will be ramped up accordingly. (Two thermocouples are wielded on the target container.)
Once at the desired temperature; the samples will be heat for 4 hours before cooling down.
Tuesday, September 17, 2013, 14:37
Target temperature has reached to 800C at around 13:00 (see attachment#2)
TGHT @ 230A/3.07V (local 233A/3.25V).
IG @ 1.06e-6 Torr.
The heater will be ramped down at ~17:00 at 2A/min.
Tuesday, September 17, 2013, 17:36
Target temp: T1 = 805C, T2=797.6C
IG @ 9.4e-7 Torr.
Cooling down initiated.
Wednesday, September 18, 2013, 11:34
TGHT at 0A. Temp at 22C.
IG @ 5.8e-7 Torr.
Venting chamber.
|
Thursday, September 19, 2013, 11:56, Laura Lambert, Nb, target boat #3 (brand new!) , , , Nb thermo treatment (Bob's samples)
|
John Wong wrote: |
Tuesday, September 17, 2013, 11:14
Target boat contains 5 Nb discs. 3 discs are wraps with 0.001" thin of Nb foil (99.8% pure), and 2 are wraps with 0.001" Ta foil (see attachment#1)
Chamber has been pumped down over night. Pressure is currently at 9.8e-7 Torr.
Heating instructions:
Samples will be heated up to 800C. TGHT will be ramped up accordingly. (Two thermocouples are wielded on the target container.)
Once at the desired temperature; the samples will be heat for 4 hours before cooling down.
Tuesday, September 17, 2013, 14:37
Target temperature has reached to 800C at around 13:00 (see attachment#2)
TGHT @ 230A/3.07V (local 233A/3.25V).
IG @ 1.06e-6 Torr.
The heater will be ramped down at ~17:00 at 2A/min.
Tuesday, September 17, 2013, 17:36
Target temp: T1 = 805C, T2=797.6C
IG @ 9.4e-7 Torr.
Cooling down initiated.
Wednesday, September 18, 2013, 11:34
TGHT at 0A. Temp at 22C.
IG @ 5.8e-7 Torr.
Venting chamber.
|
Thursday, September 19, 2013, 11:41
Target boat contains batch#2 Nb samples (see attachment #1)
Chamber has been pumped down over night.
IG @ 5.5e-07 Torr.
CG1B @ 0.033 T
CG1A @ 0.127 T
There is a leak in the backing line. BV1 was bypassed in order to turn on the turbo pump. (Will investigate the leaks after the processes are done)
*See attached picture to view samples
|
Thursday, September 19, 2013, 17:02, John Wong, Nb, target boat #3 (brand new!) , , , Nb thermo treatment (Bob's samples)
|
Laura Lambert wrote: |
John Wong wrote: |
Tuesday, September 17, 2013, 11:14
Target boat contains 5 Nb discs. 3 discs are wraps with 0.001" thin of Nb foil (99.8% pure), and 2 are wraps with 0.001" Ta foil (see attachment#1)
Chamber has been pumped down over night. Pressure is currently at 9.8e-7 Torr.
Heating instructions:
Samples will be heated up to 800C. TGHT will be ramped up accordingly. (Two thermocouples are wielded on the target container.)
Once at the desired temperature; the samples will be heat for 4 hours before cooling down.
Tuesday, September 17, 2013, 14:37
Target temperature has reached to 800C at around 13:00 (see attachment#2)
TGHT @ 230A/3.07V (local 233A/3.25V).
IG @ 1.06e-6 Torr.
The heater will be ramped down at ~17:00 at 2A/min.
Tuesday, September 17, 2013, 17:36
Target temp: T1 = 805C, T2=797.6C
IG @ 9.4e-7 Torr.
Cooling down initiated.
Wednesday, September 18, 2013, 11:34
TGHT at 0A. Temp at 22C.
IG @ 5.8e-7 Torr.
Venting chamber.
|
Thursday, September 19, 2013, 11:41
Target boat contains batch#2 Nb samples (see attachment #1)
Chamber has been pumped down over night.
IG @ 5.5e-07 Torr.
CG1B @ 0.033 T
CG1A @ 0.127 T
There is a leak in the backing line. BV1 was bypassed in order to turn on the turbo pump. (Will investigate the leaks after the processes are done)
*See attached picture to view samples
|
Thursday, September 19, 2013, 17:01
TGHT reached to 800A. Temp at 795.9C for 4 hours. Vac at 5.8e-7 Torr.
Cooling down initiated. ramping rate at 2A/min.
|
Friday, September 20, 2013, 14:59, John Wong, Nb, target boat #3 (brand new!) , , , Nb thermo treatment (Bob's samples)
|
John Wong wrote: |
Tuesday, September 17, 2013, 11:14
Target boat contains 5 Nb discs. 3 discs are wraps with 0.001" thin of Nb foil (99.8% pure), and 2 are wraps with 0.001" Ta foil (see attachment#1)
Chamber has been pumped down over night. Pressure is currently at 9.8e-7 Torr.
Heating instructions:
Samples will be heated up to 800C. TGHT will be ramped up accordingly. (Two thermocouples are wielded on the target container.)
Once at the desired temperature; the samples will be heat for 4 hours before cooling down.
Tuesday, September 17, 2013, 14:37
Target temperature has reached to 800C at around 13:00 (see attachment#2)
TGHT @ 230A/3.07V (local 233A/3.25V).
IG @ 1.06e-6 Torr.
The heater will be ramped down at ~17:00 at 2A/min.
Tuesday, September 17, 2013, 17:36
Target temp: T1 = 805C, T2=797.6C
IG @ 9.4e-7 Torr.
Cooling down initiated.
Wednesday, September 18, 2013, 11:34
TGHT at 0A. Temp at 22C.
IG @ 5.8e-7 Torr.
Venting chamber.
|
Friday, September 20, 2013, 14:56
Target contains batch#3 sample wrapped with Nb foil.
Chamber has been pumped down to 1.03e-6 Torr.
Samples will be heated up to 1200C for 4 hours.
Friday, September 20, 2013, 16:54
TGHT at 450A, temp stabilizes at 1238C.
Will cool down at 20:30 tonight.
Friday, September 20, 2013, 20:40
Samples has been heated for 4 hours at 1235C.
Cooling down initiated.
Monday, September 23, 2013, 14:40
Chamber was vented.
Batch#3 process completed.
|
Monday, September 23, 2013, 16:18, John Wong, Nb, target boat #3 (brand new!) , , , Nb thermo treatment (Bob's samples)
|
John Wong wrote: |
John Wong wrote: |
Tuesday, September 17, 2013, 11:14
Target boat contains 5 Nb discs. 3 discs are wraps with 0.001" thin of Nb foil (99.8% pure), and 2 are wraps with 0.001" Ta foil (see attachment#1)
Chamber has been pumped down over night. Pressure is currently at 9.8e-7 Torr.
Heating instructions:
Samples will be heated up to 800C. TGHT will be ramped up accordingly. (Two thermocouples are wielded on the target container.)
Once at the desired temperature; the samples will be heat for 4 hours before cooling down.
Tuesday, September 17, 2013, 14:37
Target temperature has reached to 800C at around 13:00 (see attachment#2)
TGHT @ 230A/3.07V (local 233A/3.25V).
IG @ 1.06e-6 Torr.
The heater will be ramped down at ~17:00 at 2A/min.
Tuesday, September 17, 2013, 17:36
Target temp: T1 = 805C, T2=797.6C
IG @ 9.4e-7 Torr.
Cooling down initiated.
Wednesday, September 18, 2013, 11:34
TGHT at 0A. Temp at 22C.
IG @ 5.8e-7 Torr.
Venting chamber.
|
Friday, September 20, 2013, 14:56
Target contains batch#3 sample wrapped with Nb foil.
Chamber has been pumped down to 1.03e-6 Torr.
Samples will be heated up to 1200C for 4 hours.
Friday, September 20, 2013, 16:54
TGHT at 450A, temp stabilizes at 1238C.
Will cool down at 20:30 tonight.
Friday, September 20, 2013, 20:40
Samples has been heated for 4 hours at 1235C.
Cooling down initiated.
Monday, September 23, 2013, 14:40
Chamber was vented.
Batch#3 process completed.
|
Monday, September 23, 2013, 16:14
Batch#4. Target container contains 2 Nb stables (a bullet type and a disc).
Samples are wrapped with "dimpled" Nb foil to prevent diffusion bonding.
Chamber has been pumped down to 8.3e-7 Torr, CG1B @ 30mT, CG1A @ 118mT.
Samples will be heated up to 1400C for 4 hours.
Monday, September 23, 2013, 17:46
TGHT at 620A. Temp at 1400C. Current pressure @ 2.5e-6 Torr.
Tuesday, September 24, 2013, 16:45
Sample#4 was heated up to 1400C and after about 3hrs, the target container started to break.
See the link below for more details:
https://www.dropbox.com/s/9mhpkz66u6yqldm/Nb_1400C.mp4
|
Tuesday, August 27, 2013, 17:01, John Wong, , targetboat (TaC coated), , Done, Sintering TaC coated regular caps
|
Tuesday, August 27, 2013, 16:48
Target boat is filled with TaC coated endcaps (brown) and some partial sinterred ones (gray) from before. (see attachment#1).
The container is wrapped with Ta heat-shield.
Chamber has been pumped down; IG currently @ 7.3e-7 Torr.
Heat-shield cooling water valves are open; no leaks are detected.
Initiated TGHT auto-ramping at 0.5A/min, set TGHT max at 580A.
Wednesday, August 28, 2013, 16:09
TGHT has reached to 580A and been heated for over 4 hours.
IG is coming down, currently at 1.9 e-6 Torr.
Initiated auto-cooling. 2A/min.
|
Thursday, August 29, 2013, 11:53, Laura Lambert, , targetboat (TaC coated), , Done, Sintering TaC coated regular caps
|
John Wong wrote: |
Tuesday, August 27, 2013, 16:48
Target boat is filled with TaC coated endcaps (brown) and some partial sinterred ones (gray) from before. (see attachment#1).
The container is wrapped with Ta heat-shield.
Chamber has been pumped down; IG currently @ 7.3e-7 Torr.
Heat-shield cooling water valves are open; no leaks are detected.
Initiated TGHT auto-ramping at 0.5A/min, set TGHT max at 580A.
Wednesday, August 28, 2013, 16:09
TGHT has reached to 580A and been heated for over 4 hours.
IG is coming down, currently at 1.9 e-6 Torr.
Initiated auto-cooling. 2A/min.
|
Thursday, August 29, 2013, 11:50
TGHT at 0 A
IG at 3.5e-7 Torr
Turning off EVAP2 and venting chamber
Process complete
|
Wednesday, August 21, 2013, 12:30, John Wong, Ta, 38817-10, HP-SIS, Done, Conditioning Ta target
|
Wednesday, August 21, 2013, 12:28
Container is filled with 400 discs of Ta foils, and wrapped with 3 layers of Ta heat shields.
No caps are inserted during the conditioning.
Chamber is currently being pumped down.
Wednesday, August 21, 2013, 15:54
HS cooling water valves opened, no leaks were detected.
IG @ 2.9e-6 Torr.
Heating setting:
TGHT max = 820A,
TBHT max = 230A
ramping rate 2A/min.
Thursday, August 22, 2013, 12:45
TGHT/TBHT reached to 820A/230A, respectively.
So much out-gassing was observed at the max currents. (see attachment#1).
TGHT/TBHT are ramping down at 4A/min.
Chamber will be vented in air.
The target will will be inspected.
More info later...
Thursday, August 22, 2013, 16:44
Target was removed from the evaporator and inspected.
The container and the Ta materials look OK.
The outgassing could be from the Ta-heat shields; they look burnt and brittle.
Overall, the target is good.
|
Thursday, August 08, 2013, 15:41, Laura Lambert, NiO, 39530-6, HP-FEBIAD, In progress, Sintering NiO # 2
|
Thursday, August 08, 2013, 15:19
NiO target materials loaded into the container yesterday.
Total discs = 530, (5 discs/pack)
length [after loaded] = 9.0cm
Target container is wrapped with Ta-heat shields, and will be removed after sintering process.
No end caps were inserted.
The chamber has been pumped down and currently IG1 = 3.8x10-06 Torr.
The HS cooling water was turned on and no leaks were detected.
TGHT and TBHT have been stepped up to 50A.
Auto-ramping setting:
0.2A/min for TGHT max = 250A, TBHT max = 230A.
Good vacuum = 3.00e-05 Torr
Bad vacuum = 4.00e-05 Torr
**See attachment #1 for pictures of target pre-sintering
|
Thursday, August 08, 2013, 17:28, John Wong, NiO, 39530-6, HP-FEBIAD, Done, Sintering NiO # 2
|
Laura Lambert wrote: |
Thursday, August 08, 2013, 15:19
NiO target materials loaded into the container yesterday.
Total discs = 530, (5 discs/pack)
length [after loaded] = 9.0cm
Target container is wrapped with Ta-heat shields, and will be removed after sintering process.
No end caps were inserted.
The chamber has been pumped down and currently IG1 = 3.8x10-06 Torr.
The HS cooling water was turned on and no leaks were detected.
TGHT and TBHT have been stepped up to 50A.
Auto-ramping setting:
0.2A/min for TGHT max = 250A, TBHT max = 230A.
Good vacuum = 3.00e-05 Torr
Bad vacuum = 4.00e-05 Torr
**See attachment #1 for pictures of target pre-sintering
|
Thursday, August 08, 2013, 17:26
Pressure is stabilizing at ~2.2e-5 Torr. TGHT/TBHT at 50A.
Initiated auto-ramping...
Sunday, August 11, 2013, 21:30
TGHT/TBHT have reached to 250A/230A. Target have been heated over the weekend.
Cooling down initiated; 2A/min.
The chamber wil be vented in air tomorrow.
Monday, August 12, 2013, 18:01
The sinterring process is complete.
The target is ready to be removed from the evaporator, and the endcaps will be inserted.
|
Monday, July 22, 2013, 15:03, John Wong, Empty, 38634-7, LP-SIS, Done, Sintering empty target oven coated with TaC for UCx#7
|
Monday, July 22, 2013, 15:00
Target container is coated with TaC - this container will be used for UCx#7.
Container is wrapped with 3 layers of Ta, including the back-block.
For the sintering process:
TGHT will be ramped up to 580A at 0.2A/min
TBHT will be ramped up to 230A at 0.2A/min.
Chamber has been pumped down. HS cooling H2O valves are opened, and no leaks are detected.
Currently IGP1 @ 7.03e-6 Torr.
Monday, July 22, 2013, 15:19
TGHT/TBHT was stepped up to 20A. Pressure increased to ~1.2e-5 Torr.
Auto-ramping initiated...
Wednesday, July 24, 2013, 18:40
TGHT and TBHT have reached to 580A/230A, respectively. Target has been heated for ~4 hours at that max current.
Vacuum currently at 1.65e-6 Torr.
Auto-cooling initiated... (TGHT @ -1A/min, TBHT -0.5A/min)
Target will be vented in air tomorrow.
|
Monday, June 17, 2013, 16:59, Laura Lambert, SiC, 38481-6, HP-FEBIAD, Done, Sintering of SiC #29
|
Monday, June 17, 2013, 16:57
Target is loaded with 510 SiC discs
Container was previously coated with TaC and sintered
SiC is wrapped with tantalum heat shield
Chamber is currently being pumped down
|
Tuesday, June 18, 2013, 16:40, John Wong, SiC, 38481-6, HP-FEBIAD, Done, Sintering of SiC #29
|
Laura Lambert wrote: |
Monday, June 17, 2013, 16:57
Target is loaded with 510 SiC discs
Container was previously coated with TaC and sintered
SiC is wrapped with tantalum heat shield
Chamber is currently being pumped down
|
Tuesday, June 18, 2013, 16:16
HS water valves opened; no leaks were detected.
IG @ 8.9e-7 Torr.
Note: This target has a regular end cap inserted on one end, and the other with a D-cap.
TGHT will be heated up to 820A and TBHT to 300A; ramping rate at 1A/min.
Stepped up TGHT/TBHT to 60A. Vacuum slowly increasing...
Tuesday, June 18, 2013, 17:55
Stepped up TGHT/TBTH to 80A. 10 mins later, pressure went beyond the limit and tripped of the p/s. F!
Allowed vacuum to come down below 8e-5 Torr. Stepped down TGHT/TBHT to 50A.
Currently IG @ 4.8-5 Torr.
Initiated auto-ramping: setting: Good Vac = 3e-5 Torr, Bad Vac = 4.0e-5 Torr.
Thursday, June 20, 2013, 06:21
About 10 min ago, Evap tripped off due to high vacuum.
Vacuum came back down below the trip limit and both TGHT/TBHT p/s were stepped down to 40A and turned back on.
Changed auto ramping rate to 05A/120min.
The process continues... (And I'm going back to sleep!)
Friday, June 21, 2013, 15:19
Vacuum is close to the trip limit.
Change the ramping rate to 0.2A/120min.
Monday, June 24, 2013, 17:04
Organic burnt out is complete and vacuum has come down to ~9.0e-6 Torr.
Increase ramping rate to 0.2A/60min - The sintering process should take about another 2 days if everything goes smoothly.
Wednesday, June 26, 2013, 17:29
TGHT & TBHT have reached to 820A and 300A, respectively, for 4 hours.
Vacuum is at 9e-7 Torr.
Cooling down is in progress, at a rate of 1.0A/min for TGHT and 0.5A/min for TBHT.
The target will be ready to come out by tomorrow.
Thursday, June 27, 2013, 11:02
TGHT/TBHT reached to 0A. Vacuum is leveled at 1.2e-7 Torr.
Chamber will be vented in air soon.
|
Tuesday, May 28, 2013, 17:50, John Wong, , Target Boat #2 , , Done, Sintering TaC coated end caps
|
Tuesday, May 28, 2013, 17:36
The target containers endcaps were coated with TaC solution and let dry.
Each cap is wrapped with a small piece of graphite foil and inserted in the target boat.
The chamber is currently being pumped down.
The HS cooling water valve will be opened tomorrow; any leak will be inspected.
When the vacuum is good, TGHT will be ramped up to 580A.
Wednesday, May 29, 2013, 17:06
HS water valve was opened early this morning; no leaks were detected.
TGHT has stepped up to 50A. IG is currently at 2.0e-6Torr.
Initiated auto-ramping at 1.0A/min.
Thursday, May 30, 2013, 11:12
TGHT reached to 580. The end caps have been heated at that current for more than 7 hrs.
IG is coming down, currently at 8e-7 Torr.
Auto-cooling initiated, ramping down at 2A/min .
|
Tuesday, May 14, 2013, 17:15, John Wong, Empty, 38481-6, HP-FEBIAD, Done, SinteringTaC coating
|
Tuesday, May 14, 2013, 17:04
Target oven is coated with TaC, and wrapped with 3-Ta heat shields.
TGHT and TBHT will be ramped up to 820A and 300A, respectively.
Ramping rate set to 1A/min.
Good Vac at 3.e-5 Torr, Bad Vac @ 4.0e-5 Torr.
Chamber is currently being pumped...
Wednesday, May 15, 2013, 10:56
Chamber has pumped down to 4.5e-7 Torr.
HS cooling water valves opened; no leaks were detected.
Stepping up TGHT/TBHT to 80A; monitoring vacuum.
Wednesday, May 15, 2013, 11:26
Pressure is increasing. TGHT setpoint @ 80A, readback @ 88.6A/0.603V, local @ 83A/0.80V.
Wednesday, May 15, 2013, 12:08
TGHT/TBHT stepped up to 140A and tripped off at high limit vacuum.
Restarted p/s and set TBHT/TGHT at 100A
Initiated auto ramping...
Friday, May 17, 2013, 11:39
TGHT and TBHT reached to 820A and 300A, respectively. Target has been heating at the max currents for ~12hrs.
Vacuum is coming down to 4.3e-7 Torr.
The TaC coating sintering is completed.
Autocooling is initiated. TGHT ramping rate @ 2A/min, and 1A/min for TBHT.
Wednesday, May 22, 2013, 10:43
Sintering complete.
Chamber will be vented
|
Tuesday, May 07, 2013, 16:53, Nikita Bernier, BeO, , , Done, Sintering BeO pellets #6
|
Tuesday, May 07, 2013, 16:48
5 BeO pellets were made. Each weights about 1.3 g (including org mass).
A piece of Re foil (0.002" thick) is used as the under layer to protect the reaction between Be(g) and the Ta-boat. (see Pictures)
Another layer of Ta-foil is used as the heat-shield to wrap around the Ta-boat.
The chamber was pumped down.
TGHT will be ramped up to 600 A (~1360°C) at 0.2 A/min. The vacuum limit parameter was set for good vacuum at < 3.0e-5 Torr and bad vacuum at > 4.0e0-5 Torr.
The pressure, voltage and current will be closely monitored.
If the Ta-boat survives, the TGHT will continue to ramp up to max 800 A (~1580°C).
|
Monday, May 13, 2013, 12:53, Nikita Bernier, BeO, , , Done, Sintering BeO pellets #6
|
Nikita Bernier wrote: |
Tuesday, May 07, 2013, 16:48
5 BeO pellets were made. Each weights about 1.3 g (including org mass).
A piece of Re foil (0.002" thick) is used as the under layer to protect the reaction between Be(g) and the Ta-boat. (see Attachments)
Another layer of Ta-foil is used as the heat-shield to wrap around the Ta-boat.
The chamber was pumped down.
TGHT will be ramped up to 600 A (~1360°C) at 0.2 A/min. The vacuum limit parameter was set for good vacuum at < 3.0e-5 Torr and bad vacuum at > 4.0e0-5 Torr.
The pressure, voltage and current will be closely monitored.
If the Ta-boat survives, the TGHT will continue to ramp up to max 800 A (~1580°C).
|
Monday, May 13, 2013, 12:48
TGHT has been at 600 A for about 13 hours with stable very low vacuum (10^-7). See Attachment #1.
Temperature measurement has been lost on Saturday. Last measurement was was above 1350°C, at around 480 A.
TGHT was ramped down at 1 A/min.
The chamber will be vented later today. The pellets and the thermocouples will be inspected.
|
Monday, May 13, 2013, 17:17, Nikita Bernier, BeO, , , Done, Sintering BeO pellets #6
|
Nikita Bernier wrote: |
Nikita Bernier wrote: |
Tuesday, May 07, 2013, 16:48
5 BeO pellets were made. Each weights about 1.3 g (including org mass).
A piece of Re foil (0.002" thick) is used as the under layer to protect the reaction between Be(g) and the Ta-boat. (see Attachments)
Another layer of Ta-foil is used as the heat-shield to wrap around the Ta-boat.
The chamber was pumped down.
TGHT will be ramped up to 600 A (~1360°C) at 0.2 A/min. The vacuum limit parameter was set for good vacuum at < 3.0e-5 Torr and bad vacuum at > 4.0e0-5 Torr.
The pressure, voltage and current will be closely monitored.
If the Ta-boat survives, the TGHT will continue to ramp up to max 800 A (~1580°C).
|
Monday, May 13, 2013, 12:48
TGHT has been at 600 A for about 13 hours with stable very low vacuum (10^-7). See Attachment #1.
Temperature measurement has been lost on Saturday. Last measurement was was above 1350°C, at around 480 A.
TGHT was ramped down at 1 A/min.
The chamber will be vented later today. The pellets and the thermocouples will be inspected.
|
Monday, May 13, 2013, 17:21
The following table shows the characteristics of the pellets after sintering at 600 A for 13 hours.
Sample, Mass (g), Thickness (mm), Density (g/cm3), Diameter (mm)
1 0.8904 4.875 1.364 13.058
2 0.8991 4.744 1.396 13.148
3 0.8846 4.579 1.482 12.884
4 0.9142 4.981 1.254 13.650
5 0.9022 4.978 1.250 13.586
Avg 0.8981 4.831 1.345 13.265
All pellets are rugged and slightly greyish. They will be sintered up to 800 A when the thermocouples get replaced.
|
Tuesday, April 30, 2013, 11:20, Anders Mjos, Empty, 38481-5, HP-FEBIAD, Done, CTL thermal test
|
CTL block on T/C F/T Ch 1
Supply on Ch 3
HS Return on Ch 4
Tuesday, April 30, 2013, 11:20: Roughing
Tuesday, April 30, 2013, 11:45: Turbo started
Wednesday, May 01, 2013, 08:43: Cooling water opened. Vacuum stable at 5.1E-7 T (IGP1)
Wednesday, May 01, 2013, 08:48: Ramping TGHT and TBHT to 850A and 300A at 1A/60s
Thursday, May 02, 2013, 09:10: TGHT reached voltage limit (12V) at ~780A yesterday at ~10pm. Increased limit to 12.5V and continued auto ramping. CTL block temp ~80C
Thursday, May 02, 2013, 10:08: TGHT voltage limit changed to 13V. TGHT:RDCUR goes to ~810A with TGHT:RDVOL at 12.5V. CTL block temp ~80C
Thursday, May 02, 2013, 11:33: TGHT manually stepped to 850A RDCUR at 846A, RDVOL at 13.1V. CTL block temp ~84C
Thursday, May 02, 2013, 15:13: Ramping down TGHT and TBHT to 580A and 280A at 2A/min and 1A/min
Friday, May 03, 2013, 08:30: TGHT and TBHT at 580A and 280A. CTL block temp ~60C
Friday, May 03, 2013, 08:37: Ramping down TGHT and TBHT to 0 at 2/min and 1A/min
Friday, May 03, 2013, 11:04: T/C logger removed
Monday, May 06, 2013, 09:37: Turbo stopped.
Monday, May 06, 2013, 10:26: Venting |
Friday, April 19, 2013, 15:27, Anders Mjos, Empty, 38481-4, HP-FEBIAD, Done, CTL test
|
Target installed with 4 T/C
The target assembly is ITD0300 with the CTL Cu cooling block slightly modified.
Ch1 - CTL cooling block T/C feedtrough
Ch2 - Heat shield below left gripper arm - T/C feedthrough
Ch3 - Heat shield below left gripper arm - 9 pin connector
Ch4 - Target left side leg on tube - 9 pin connector
Friday, April 19, 2013, 15:23: Roughing
Friday, April 19, 2013, 15:41: Started turbo
Monday, April 22, 2013, 09:43: Opened water supply. Vacuum stable at 2.8E-7 T (IGP1) |
Monday, April 22, 2013, 18:49, John Wong, Empty, 38481-4, HP-FEBIAD, Done, CTL test
|
Anders Mjos wrote: |
Target installed with 4 T/C
The target assembly is ITD0300 with the CTL Cu cooling block slightly modified.
Ch1 - CTL cooling block T/C feedtrough
Ch2 - Heat shield below left gripper arm - T/C feedthrough
Ch3 - Heat shield below left gripper arm - 9 pin connector
Ch4 - Target left side leg on tube - 9 pin connector
Friday, April 19, 2013, 15:23: Roughing
Friday, April 19, 2013, 15:41: Started turbo
Monday, April 22, 2013, 09:43: Opened water supply. Vacuum stable at 2.8E-7 T (IGP1)
|
Monday, April 22, 2013, 18:48
Ramping TGHT/TBHT to 850A/300A at 1A/min.
|
Tuesday, April 23, 2013, 10:11, Anders Mjos, Empty, 38481-4, HP-FEBIAD, Done, CTL test
|
John Wong wrote: |
Anders Mjos wrote: |
Target installed with 4 T/C
The target assembly is ITD0300 with the CTL Cu cooling block slightly modified.
Ch1 - CTL cooling block T/C feedtrough
Ch2 - Heat shield below left gripper arm - T/C feedthrough
Ch3 - Heat shield below left gripper arm - 9 pin connector
Ch4 - Target left side leg on tube - 9 pin connector
Friday, April 19, 2013, 15:23: Roughing
Friday, April 19, 2013, 15:41: Started turbo
Monday, April 22, 2013, 09:43: Opened water supply. Vacuum stable at 2.8E-7 T (IGP1)
|
Monday, April 22, 2013, 18:48
Ramping TGHT/TBHT to 850A/300A at 1A/min.
|
Tuesd ay, April 23, 2013, 10:07
TBHT / TGHT: 820A / 300A
TGHT:RDCUR: 816.6A
TBHT:RDCRU: 303.5A
Local P/S displays
TGHT: 821A / 11.05V
TBHT: 307A / 4.37V
Tuesday, April 23, 2013, 10:45: Ramping down TBHT to 0A @ 5A/min
Tuesday, April 23, 2013, 12:49: Ramping down TGHT to 0A @ 5A/min
Tuesday, April 23, 2013, 15:52: Swithced off TGHT and TBHT P/S. TGHT P/S showed 30A read back value, while local value was 0A
Wednesday, April 24, 2013, 09:53: Turbo stopped
Wednesday, April 24, 2013, 12:00: Target removed
The ionizer tube was found to have deformed as seen in the attached photo. |
Friday, April 19, 2013, 09:39, Rick Maharaj, Empty, , , Done, thermocouple Feedthru
|
A thermocouple feedthru was installed via 9 pin sub-D connector. It runs from the the conflat cross on the top of the evaporator to the upper 9 pin connector of the target mounting plate. |
Thursday, April 11, 2013, 14:20, John Wong, Empty, 39165-6, LP-SIS, Done, Coating target oven /w TaC & sintering for UCx#6
|
Monday, April 08, 2013, 17:39
Target container is coated with TaC; the container will be used for the UCx#6 target.
No Ta-heat shields are used.
For the sintering process:
TGHT will be ramped up to 580A at 0.2A/min
TBHT will be ramped up to 230A at 0.2A/min
Chamber has been pumped down. HS cooling H2O valve opened; no leaks have detected.
Thursday, April 11, 2013, 14:35
Target and tube heaters have reached to optimum.
Auto-cooling initiated...
Friday, April 12, 2013, 11:17
P/S off. Chamber vented.
Done!
|
Thursday, March 14, 2013, 12:27, Anders Mjos, Empty, 38481-4, HP-FEBIAD, Done, CTL thermal test 3 (w/o CTL block)
|
Thursday, March 12, 2013
The CTL was removed and target heated to 580A / 300A
T1: Left target leg close to tube
T2: Heat Shield above CTL
T3: Heat Shield cooling water Supply
T4: Heat Shield cooling water Return
Thursday, March 13, 2013
The target was cooled down
Results attached as PDF and Excel |
Wednesday, March 13, 2013, 16:08, Anders Mjos, Empty, 38481-4, HP-FEBIAD, Done, Thermal test
|
Wednesday, March 13, 2013
Thermocouple channels (see attached PDF for photos)
T1 - Left target leg at tube
T2 - Between cooling fins close to tube, left side
T3 - Supply water HS
T4 - Return water HS
Friday, March 22, 2013
Test not conducted. Target removed. |
Wednesday, March 06, 2013, 10:41, Anders Mjos, Empty, 38481-4, HP-FEBIAD, Done, CTL thermal test
|
Wednesday, March 06, 2013
The Cool Transfer Line (CTL) test target is installed for thermal tests. Drawing number is ITD0431 REV A.
Thermocouple channels are as follows:
T1: Cu block on CTL
T2: Heat Shield above CTL
T3: Heat Shield cooling water Supply
T4: Heat Shield cooling water Return
Cooling water is in Evap2 supplied to the cooling line that goes directly to the area on the Heat Shield above the CTL.
Test results attached.
|
Wednesday, March 06, 2013, 17:53, John Wong, Empty, 38481-4, HP-FEBIAD, Done, CTL thermal test
|
Anders Mjos wrote: |
Wednesday, March 06, 2013
The Cool Transfer Line (CTL) test target is installed for thermal tests. Drawing number is ITD0431 REV A.
Thermocouple channels are as follows:
T1: Cu block on CTL
T2: Heat Shield above CTL
T3: Heat Shield cooling water Supply
T4: Heat Shield cooling water Return
Cooling water is in Evap2 supplied to the cooling line that goes directly to the area on the Heat Shield above the CTL.
|
Wednesday, March 06, 2013, 17:23
The target has been pumping down to 5.3 e-7 Torr. On the RGA mass scan, mainly H2O (mass 18 + constituents) was detected at ~2.7pA (see attachment #1).
The target will be heated up: TGHT = 850A (rate @ 1A/min); TBHT = 300A (rate @ 1A/min).
Thursday, March 07, 2013, 11:51
TGHT and TBHT reached to 850A (local, 845A\13.80V) and 300A, respectively. The out gassing of CO (mass 28) reached to ~5pA at the max currents. (see attachment #2)
TBHT will be ramped down to 0A to compare the temperatures.
Thursday, March 07, 2013, 15:55
TBHT at 0A. See attachment#3 for the temperatures and RGA data before further ramping down the TGHT.
|
Monday, March 11, 2013, 12:23, Anders Mjos, Empty, 38481-4, HP-FEBIAD, Done, CTL thermal test 2
|
Anders Mjos wrote: |
Wednesday, March 06, 2013
The Cool Transfer Line (CTL) test target is installed for thermal tests. Drawing number is ITD0431 REV A.
Thermocouple channels are as follows:
T1: Cu block on CTL
T2: Heat Shield above CTL
T3: Heat Shield cooling water Supply
T4: Heat Shield cooling water Return
Cooling water is in Evap2 supplied to the cooling line that goes directly to the area on the Heat Shield above the CTL.
|
Monday, March 11, 2013
The CTL test target was installed again for a second thermal test. CTL block fastened to HS with 1 in lbs. A small piece of Ta-foil of 0.001" thickness was used between the CTL Cu-block and the Ta transfer line to reduce the heat transfer..
Thermocouples were re-attached to CTL and Heat Shield (see above for channels #s).
See attached graph (PDF) for details. |
Monday, March 11, 2013, 15:59, John Wong, Empty, 38481-4, HP-FEBIAD, Done, CTL thermal test 2
|
Anders Mjos wrote: |
Anders Mjos wrote: |
Wednesday, March 06, 2013
The Cool Transfer Line (CTL) test target is installed for thermal tests. Drawing number is ITD0431 REV A.
Thermocouple channels are as follows:
T1: Cu block on CTL
T2: Heat Shield above CTL
T3: Heat Shield cooling water Supply
T4: Heat Shield cooling water Return
Cooling water is in Evap2 supplied to the cooling line that goes directly to the area on the Heat Shield above the CTL.
|
Monday, March 11, 2013
The CTL test target was installed again for a second thermal test. CTL block fastened to HS with 1 in lbs. A small piece of Ta-foil of 0.001" thickness was used between the CTL Cu-block and the Ta transfer line to reduce the heat transfer..
Thermocouples were re-attached to CTL and Heat Shield (see above for channels #s).
|
Monday, March 11, 2013, 15:55
Chamber was pumped down to 2 e-7 Torr. HS water valve opened and no leaks were detected.
TGHT and TBHT are ramping up to 850A and 300A at 2A/min, respectively.
RGA is running...
Tuesday, March 12, 2013, 10:44
TGHT/TBHT reached to max currents.
See attachment #1 for temperature and RGA measurements.
Cooling down in process... 5A/min.
|
Monday, March 04, 2013, 17:41, John Wong, Empty, LP-SIS RFQ ver 2.0, , , Testing LPSIS RFQ ver 2.0
|
Monday, March 04, 2013, 17:39
This is the 2nd modified target container for RFQ LPSIS. The container will be heated up to 650A TGHT and 150A on TBHT. No Ta-heat shield is being used.
Heating rate at 1A/min for both TGHT & TBHT. Once the target is at the currents, TBHT will be further ramped up to 300A.
Temperatures are being measured by two thermocouples (one on RFQ component and the other on the Cu heat-shield).
Gases are being analyzed using the RGA.
|
Friday, February 22, 2013, 15:55, John Wong, SiC, , LP-SIS, Done, Sintering SiC#28-RFQ
|
Friday, February 22, 2013, 15:49
The LP-SIS RFQ target container was previously coated with TaC and sintered up to ~1500C (TGHT @ 600A, TBHT @ 300A).
The container is loaded with 325 discs of SiC, a total of 10.9cm in length.
For this process,
TGHT will be ramped up to 600A and at the same time TBHT will go up to 300A. No Ta-heat shield is used.
The ramping rate is set to 0.2A/min.
The chamber is currently being pumped down.
Friday, March 01, 2013, 15:57
The target was further heated up to 650A TGHT and 300A TBHT for 4 hours yesterday; then it was cooled down.
Some reactions on the target end (where the D-cap inserted) was observed.
Yellow crystals on the D-cap was formed, just as we have seen before.
Overall, the target looks good!
See attachment#2 for the target production.
More about the gasses analyst from the RGA later...
|
Monday, February 18, 2013, 16:43, John Wong, Empty, , LP-SIS, Done, Sintering TaC coating on the RFQ target container
|
Monday, February 18, 2013, 16:28
The RFQ target container is coated with TaC and ready to be sintered. No Ta-heat shields are used. This container will be used for the SiC#28-LPSIS-RFQ.
Two thermocouples are welded on the container: One on the end cap and the other on the back block (see attachment#1)
The target will be heated to at least TGHT at 580A and TBHT at 300A; the vacuum and gasses will be monitored.
The chamber is currently being pumped down...
Friday, February 22, 2013, 14:24
The gasses were analyzed with the RGA:
TGHT @ 520A, TBHT @ 300A: Mass 28 (CO) reached to max current of ~5pA before the current started to decrease, (see attachment #2). This could be the indication of the material(s) in the target container was "sort of" fully reduced.
TGHT was further ramped up to 600A and heated for a few hours. The temperature on the end was measured at 1252C and the center block was at 1580C. (see attachment #3).
The container was successfully sintered with TaC.
|
Tuesday, January 22, 2013, 16:14, John Wong, , , LP-SIS, Done, Heating RFQ components & measuring temperatures
|
Tuesday, January 22, 2013, 12:38
This is to test the newly developed RFQ target to be commissioned this year. The purpose of this test is to see how well the RFQ components can sustain the high temperature. One thermocouple is connected inside the target and the other is connect outside of the Cu heat-shield. RGA will be running to analyze the gasses.
TGHT will be auto-ramped up at the rate of 5A/20min to max current at 1000A.
More info later...
Wednesday, February 06, 2013, 16:11
Heat testing Test#1 complete. Data acquisition in progress.... The test was successful.
Re-heating Test#2 is in progress. This time, with a new re-design target container (less black block mass). Two thermocouples are connected: One on the back block and the other inside the RFQ components.
The TGHT current will go up to at least 580A and the gasses will be monitored with the RGA. Ramping rate: 0.5A/min. Set final current at 400A for now.
TBHT will remain off at this point until we can know the temperature when TGHT is up to 580A.
Thursday, February 07, 2013, 11:39
TGHT reached to 400A/6.30V.
Back block temperature measured at 18.307mV = 1003 C.
RFQ component temperature measured at = 143 C.
TGHT will be ramped up to 580A.
Continue to monitor...
Saturday, February 09, 2013, 09:40
TGHT at 580A, TBHT at 271A (setpoint). Seeing CO2 gassing out. Ramped down TBHT to zero A and continue to monitor.
Tuesday, February 12, 2013, 16:39
TGHT heated up to 580A and remained at that current over the long weekend.
The thermocouple on the back block was reading wrong because the wires away from the tip were fused to the container at high current. (see attachment #1)
TBHT was ramped up to 300A and then lower to 280A; mass 32 (CH3OH), and 44 (CO2) were detected. This is unusual at 580A = 1200C.
Both TBHT and TGHT were ramped down to zero and the outgassing of these molecules continue to detect on the RGA. (see attachment #2). Suspect of these gasses from the Cu heat-shield or the thermocouple SiO insulator.
For complete process on screenshots, see my dropbox.
Next: Coat this container with TaC and use for the SiC target.
|
Friday, January 11, 2013, 11:16, John Wong, , , , Maintenance, Replace terminal insulator
|
Friday, January 11, 2013, 10:59
The insulator that holds the terminals was broken when a target container was installed. The insulator had seen so much heat shine from the Cu heat-shield gaps, see attachment. Tightening the bolts on the target container might further put more force on the insulator and eventually broke it.
To prevent this to happen again. The Cu-heat shield gaps have covered with Ta-foil to prevent any shine from the target container onto the insulator. Also, a torque wrench will be used to tighten the bolts on the terminals. At this point, we don't know the max torque the insulator can tolerate. Some measurements were done on the target resistant (ohm) as a function of torque (in pounds). The best torque to tighten the terminal bolts is 150 lbs.
|
Friday, January 11, 2013, 15:16, Anders Mjos, , , , Maintenance, Replace terminal insulator
|
John Wong wrote: |
Friday, January 11, 2013, 10:59
The insulator that holds the terminals was broken when a target container was installed. The insulator had seen so much heat shine from the Cu heat-shield gaps, see attachment. Tightening the bolts on the target container might further put more force on the insulator and eventually broke it.
To prevent this to happen again. The Cu-heat shield gaps have covered with Ta-foil to prevent any shine from the target container onto the insulator. Also, a torque wrench will be used to tighten the bolts on the terminals. At this point, we don't know the max torque the insulator can tolerate. Some measurements were done on the target resistant (ohm) as a function of torque (in pounds). The best torque to tighten the terminal bolts is 150 lbs.
|
The insulators were installed with torques as indicated in the attached PDF ITD0052. A torque test was performed on the broken insulator before installation. No damage was seen on torques of up to 60 in lbs for the 1/4-20 bolts, however for torques in excess of 50 in lbs the insulator material seems to "give". |
Friday, January 11, 2013, 14:00, John Wong, Empty, Ta-Target boat, , Done, Testing QMS & thermocouples
|
Friday, January 11, 2013, 13:52
TEST#1
A new target boat is coated with TaC and will go through the sintering process at 580A (max). Ramping rate 5A/20min.
For this test, two thermocouples are installed to measure the temperature of the container. The QMS is also operating to analyze the gases.
See attachment#1 for the thermocouple setup. Note: No Ta heat shield is used to wrap around the target container.
See attachment#2 for an example of the QMS and temperature measurements.
More details about the results later...
Tuesday, January 22, 2013, 12:19
The test was successfully complete.
Short summary of the results:
1. A significant difference in the temperature dependence on the heater current could be found when ramping up/down (see attachment #3).
2. A difference of 200 C at the highest temperature was between the two thermocouples were measured.
3. The measured temperatures are lower than previous measurements with a pyrometer on an empty LP target container (see attachment#3).
4. RGA spectra show most of the higher mass organic molecules are gone after initial heating at low temperature.
5. Above 560A, CO2 shows up again and decreases up to about 680A heating current. (see attachment #4).
6. After running at high temperature for some time, only H2O & CO and their constituents are left. (see attachment #5).
Data can be found on my dropbox, folder "RFQ-test\Test#1-ver1.0"
Next: Re-heating the target
Tuesday, February 12, 2013, 17:10
TEST#2: Re-heating the target again. See if it fit the curves. Measuring concentrations of 14N, 16O, 18H2O, 28CO, 32 CH3OH, 40Ar, 44C02.
Ramping rate 1A/min
Wednesday, March 06, 2013, 18:14
Test#2 complete. Data can be found on my dropbox, folder "RFQ-test\Test#2-ver1.0"
Wednesday, March 06, 2013, 18:14
Test#3: RFQ target container_version 2.0, thermal test.
Measuring back block temperature & analyze gases.
Data can be found on my dropbox, folder "RFQ-test\Test#3-ver2.0"
|
Tuesday, October 16, 2012, 14:18, John Wong, TiC, 39165-4, LP-SIS, Done, Sintering TiC#3
|
Tuesday, October 16, 2012, 14:12
Target is filled with 360 discs of TiC (with 1 mole of graphite) backed on C-grv foil.
No Ta heat-shields wrapped around the container.
One regular end-cap is inserted and expanded. The other end is inserted with a D-cap for out-gassing.
Re ionizer foil is inserted.
TGHT will be ramped up to 580A, TBHT to 230A; ramping rate at 0.2A/min.
Chamber is currently being pumped down...
Tuesday, October 16, 2012, 16:11
HS water valve is opened. No leaks is detected.
Vacuum is coming down steadily. IGP1 currently at 1.7e-5 Torr.
Wednesday, October 17, 2012, 11:41
The chamber was pumped down overnight. IGP1 reads at 5.8e-7 Torr.
Both TGHT & TBHT were stepped up to 30A. P/S OK!
Initiated auto-ramping...
Monday, October 22, 2012, 10:58
TGHT and TBHT have reached to 580A & 230A, respectively (see attachment#1).
IGP1 currently at 6.27e-6 Torr. BP@20mTorr.
Currents will remain at max for another 3 hours.
Local temperature measured at 1500C (container surface), 1300C (center block)
Monday, October 22, 2012, 17:27
Auto cooling initiated.
Tuesday, October 23, 2012, 17:54
TGHT & TBHT are at 0A. P/S & pumps off.
The chamber will be vented, and the target will be taken out for inspections.
|
Wednesday, October 10, 2012, 16:37, John Wong, Empty, 39165-4, LP-SIS, Done, Coating target oven /w TaC & sintering for TiC#3
|
Wednesday, October 10, 2012, 16:35
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min.
TBHT will be ramped up to 230A at 0.2A/min.
Chamber is currently being pumped down
Wednesday, October 10, 2012, 17:31
Chamber was pumped down to mid 10-6 Torr. HS water valve was opened and no leak in vacuum was observed.
TGHT and TBHT were stepped up to 30A. Everything seems fine...
Initiated auto-ramping: Good vac = 2.0e-5 torr, Bad Vac = 3.0e-5 Torr.
Thursday, October 11, 2012, 10:35
TBHT has reached to 230A, 3.52V.
TGHT has reached to 232A. Vacuum is stabilizing at 8.0e-7 Torr, BP at 19 mTorr.
Increased TGHT ramping rate to 2.0A/min.
Thursday, October 11, 2012, 14:55
TGHT reached to 580A/9.95V, local 575A/10.03V.
TGHT at 230A/3.62V
Local target container temperature measured at ~1430C, central block at ~1220C
IGP1 currently at 1.68e-6 Torr.
Heaters will be remained on for another 2 hours or so before auto-cooling is initiated.
Thursday, October 11, 2012, 17:49
Target container has been heated for over 4 hrs.
IGP1 @ 1.10e-6 Torr, BP @ 18mTorr
Auto-cooling initiated, rate @ 2A/min.
Friday, October 12, 2012, 10:02
TBHT/TGHT have reached to zero current.
P/S off.
Venting chamber..
see attachment#1: striptool archiver
Tuesday, October 16, 2012, 10:35
Container looks good. It will be used for TiC#3
|
Wednesday, September 26, 2012, 15:14, Nikita Bernier, BeO, , , Done, Sintering BeO Pellets #4
|
Wednesday, September 26, 2012, 15:07
The samples were made of BeO powder with 30% PVB which was treated at 400 RPM for 26 minutes. A ratio of 10:1 of mineral oil was added before another high speed treatment for 10 minutes. The powder was then pressed into pellets.
Three pellets were loaded on the target boat coated with TaC, with an extra layer of TaC coated Ta foil. See Attachment 1. The target boat is wrapped with a Ta foil that is 0.002 inches thick.
Target chamber was pumped down. The cooling water was turned on and no leak were observed.
TGHT was stepped up to 55A before the auto ramping was initiated at 0.5 A/min. The vacuum limit parameter was set for good vac at <3.0 e-5 Torr and bad vac at >4.0 e0-5 Torr.
|
Friday, September 28, 2012, 12:59, Nikita Bernier, BeO, , , Done, Sintering BeO Pellets #4
|
Nikita Bernier wrote: |
Wednesday, September 26, 2012, 15:07
The samples were made of BeO powder with 30% PVB which was treated at 400 RPM for 26 minutes. A ratio of 10:1 of mineral oil was added before another high speed treatment for 10 minutes. The powder was then pressed into pellets.
Three pellets were loaded on the target boat coated with TaC, with an extra layer of TaC coated Ta foil. See Attachment 1. The target boat is wrapped with a Ta foil that is 0.002 inches thick.
Target chamber was pumped down. The cooling water was turned on and no leak were observed.
TGHT was stepped up to 55A before the auto ramping was initiated at 0.5 A/min. The vacuum limit parameter was set for good vac at <3.0 e-5 Torr and bad vac at >4.0 e0-5 Torr.
|
Friday, September 28, 2012, 12:50
Sintering was coming up smoothly. As expected, resistance started building up quickly at higher temperatures (above 600°C). See Attachment 1. The target heater tripped off twice this morning. I was able to ramp up the current after the first trip until it tripped again. After the second time, the voltage went crazy and I had to ramp down the current. Attachment 2 shows the whole process.
Evap2 will be vented out shortly and the pellets will be examined.
Friday, September 28, 2012, 15:52
The boat comes in two parts. One pellet is missing. The two remaining pellets are black and grey. Also they shrank a lot. See Attachment 3.
So once again, a new batch of BeO pellets will have to be prepared and sintered in order to determine the dimensions of the final die. Therefore the best approach is still loading the pellets on a target boat coated/sintered with TaC and wrapped with a Ta foil.
|
Monday, September 24, 2012, 15:12, Nikita Bernier, TaC, , , Done, Sintering Ta foil with TaC coating
|
Monday, September 24, 2012, 15:01
The target boat with TaC coating is being used again. The inside of the boat is covered with a 0.002 inches thick Ta foil with TaC coating, wrapped with a 0.002 inches thick Ta foil.
Chamber was pumped down to 6e-6 Torr before the Heat Shield cooling water valve was opened. A small vacuum bump was detected (See attachment #1). It is not clear if it was caused by a water leak or not.
After consulting with Peter, I will wait for the vacuum to be below e-07 Torr before turning the target heater on.
|
Monday, September 24, 2012, 18:09, Nikita Bernier, TaC, , , Done, Sintering Ta foil with TaC coating
|
Nikita Bernier wrote: |
Monday, September 24, 2012, 15:01
The target boat with TaC coating is being used again. The inside of the boat is covered with a 0.002 inches thick Ta foil with TaC coating, wrapped with a 0.002 inches thick Ta foil.
Chamber was pumped down to 6e-6 Torr before the Heat Shield cooling water valve was opened. A small vacuum bump was detected (See attachment #1). It is not clear if it was caused by a water leak or not.
After consulting with Peter, I will wait for the vacuum to be below e-07 Torr before turning the target heater on.
|
Monday, September 24, 2012, 18:02
The vacuum was stable until 1e-06 Torr. The target heater was turned on and tapped up to 60 A (0.8 V).
Evaporator #2 is now auto-ramping overnight at 0.2 A/min, up to 800-850 A, with the maximum voltage limited at 14 V, between 2.00e-05 (Good vacuum) and 3.00e-05 Torr (Bad vacuum).
Tuesday, September 25, 2012, 15:11
Sintering process is going smoothly. See Attachment 1. The auto-ramping was increased to 1 A/min up to 800-850 A.
Tuesday, September 25, 2012, 16:11
And the voltage limit was increased to 18 V ! See Attachment 2.
Tuesday, September 25, 2012, 19:13
Around 806 A (readback), voltage increased more quickly than the current. It seems like resistance is building up. After reaching 836 A (readback), the current was tapped down to 800 A (readback)/ 816 A (setting) in an effort to save the Ta boat. See Attachment 3. The current will stay at 800 A for ~4 hours before ramping down.
|
Wednesday, September 26, 2012, 15:06, Nikita Bernier, TaC, , , Done, Sintering Ta foil with TaC coating
|
Nikita Bernier wrote: |
Nikita Bernier wrote: |
Monday, September 24, 2012, 15:01
The target boat with TaC coating is being used again. The inside of the boat is covered with a 0.002 inches thick Ta foil with TaC coating, wrapped with a 0.002 inches thick Ta foil.
Chamber was pumped down to 6e-6 Torr before the Heat Shield cooling water valve was opened. A small vacuum bump was detected (See attachment #1). It is not clear if it was caused by a water leak or not.
After consulting with Peter, I will wait for the vacuum to be below e-07 Torr before turning the target heater on.
|
Monday, September 24, 2012, 18:02
The vacuum was stable until 1e-06 Torr. The target heater was turned on and tapped up to 60 A (0.8 V).
Evaporator #2 is now auto-ramping overnight at 0.2 A/min, up to 800-850 A, with the maximum voltage limited at 14 V, between 2.00e-05 (Good vacuum) and 3.00e-05 Torr (Bad vacuum).
Tuesday, September 25, 2012, 15:11
Sintering process is going smoothly. See Attachment 1. The auto-ramping was increased to 1 A/min up to 800-850 A.
Tuesday, September 25, 2012, 16:11
And the voltage limit was increased to 18 V ! See Attachment 2.
Tuesday, September 25, 2012, 19:13
Around 806 A (readback), voltage increased more quickly than the current. It seems like resistance is building up. After reaching 836 A (readback), the current was tapped down to 800 A (readback)/ 816 A (setting) in an effort to save the Ta boat. See Attachment 3. The current will stay at 800 A for ~4 hours before ramping down.
|
Wednesday, September 26, 2012, 14:31
The current was tapped down twice as resistance was building up. After 4 hours at ~800 A, the TGHT was ramped down at 2 A/min. See Attachment 1. The target boat was cooled down for 4 hours before the chiller was turned off.
Also I had trouble measuring the temperature. I was unable to get a clear picture with the pyrometer. Therefore the exact temperature remains unknown, but from previous experiments, 800 A was about 1400°C.
The TaC coated Ta foil is very brittle. There is a lot of crystallisation on the Ta boat. See attachment 2. It is unlikely that the boat would survive many more sintering. Therefore it will be used for BeO pellets tests.
When John gets back, I suggest we use a new boat coated with TaC, without additional layers. (See message #15 when this target boat was sintered up to 900A (local 893A/16.88V), Measured temp @ 1500°C)
|
Wednesday, August 22, 2012, 17:36, John Wong, Empty, 39165-5, LP-SIS, Done, Coating target oven /w TaC & sintering for UCx#5
|
Wednesday, August 22, 2012, 17:25
Note: LP-FEBIAD target container ( W.O#37918-3) was coated with TaC and sintered on July 19 for UCx#5 target. Then, a last minute request from the Sci Dev. to run the UCx#5 in LP-SIS.
The target container was coated with TaC (Using IR heat lamp to speed the drying time)
It's wrapped with 3 layers of Ta as the heat-shield, including the backblock.
TGHT will be ramped up to 580A at 0.5A/min.
TBHT will be ramped up to 230A at 0.5A/min.
Chamber is currently being pumped down.
Wednesday, August 22, 2012, 18:27
Chamber was pumped down to 5.4e-6 Torr; the HS cooling water valve was opened and no leaks were detected.
Stepped up TGHT/TBHT to 20A.
Initiated auto-ramping...
Friday, August 24, 2012, 00:21
TGHT/TBHT have reached to 580A/230A, respectively, and have remained at the currents for ~10hrs.
Current, IG1 is at 9.3e-7 torr. The sintering process is done.
Initiating auto-cool down at 2A/min.
Friday, August 24, 2012, 13:31
TGHT & TBHT power supplies are off.
The chamber is vented.
|
Friday, August 10, 2012, 19:57, Nikita Bernier, , , , Done, Sintering Ta foil with TaO coating
|
Friday, August 10, 2012, 19:54
Target boat with TaC coating, inside covered with a 0.002 inches thick Ta foil, wrapped with a 0.002 inches thick Ta foil, contains a Ta foil with TaO coating.
See John's Ipad for their recipes.
Evaporator #2 is now auto-ramping overnight at 0.2 A/min, up to 830 A, with the maximum voltage limited at 14 V, between 2.00e-05 (Good vacuum) and 3.00e-05 Torr (Bad vacuum).
|
Saturday, August 11, 2012, 19:21, Nikita Bernier, , , , Done, Sintering Ta foil with TaO coating
|
Nikita Bernier wrote: |
Friday, August 10, 2012, 19:54
Target boat with TaC coating, inside covered with a 0.002 inches thick Ta foil, wrapped with a 0.002 inches thick Ta foil, contains a Ta foil with TaO coating.
See John's Ipad for their recipes.
Evaporator #2 is now auto-ramping overnight at 0.2 A/min, up to 830 A, with the maximum voltage limited at 14 V, between 2.00e-05 (Good vacuum) and 3.00e-05 Torr (Bad vacuum).
|
Saturday, August 11, 2012, 19:15
Heating process was going smoothly up to 400 A. See Attachment 1.
Around 420 A, vacuum went up again and the voltage increased more quickly. It seems like resistance is building up. After reaching 530 A, the current was tapped down to 420 A in an effort to save the Ta boat. See Attachment 2.
The current will stay at 420 A for the weekend until John takes a look at this.
|
Monday, August 13, 2012, 13:50, Nikita Bernier, , , , Done, Sintering Ta foil with TaO coating
|
Nikita Bernier wrote: |
Nikita Bernier wrote: |
Friday, August 10, 2012, 19:54
Target boat with TaC coating, inside covered with a 0.002 inches thick Ta foil, wrapped with a 0.002 inches thick Ta foil, contains a Ta foil with TaO coating.
See John's Ipad for their recipes.
Evaporator #2 is now auto-ramping overnight at 0.2 A/min, up to 830 A, with the maximum voltage limited at 14 V, between 2.00e-05 (Good vacuum) and 3.00e-05 Torr (Bad vacuum).
|
Saturday, August 11, 2012, 19:15
Heating process was going smoothly up to 400 A. See Attachment 1.
Around 420 A, vacuum went up again and the voltage increased more quickly. It seems like resistance is building up. After reaching 530 A, the current was tapped down to 420 A in an effort to save the Ta boat. See Attachment 2.
The current will stay at 420 A for the weekend until John takes a look at this.
|
Monday, August 13, 2012, 13:46
TGHT was ramped down at 2 A/min and then tapped down to 0A. See Attachment 1. The target boat will be cooled down for about an hour before turning off the chiller.
|
Tuesday, August 14, 2012, 17:11, John Wong, , , , Failed, Sintering Ta2O5 coating on Ta foil failed
|
Nikita Bernier wrote: |
Nikita Bernier wrote: |
Nikita Bernier wrote: |
Friday, August 10, 2012, 19:54
Target boat with TaC coating, inside covered with a 0.002 inches thick Ta foil, wrapped with a 0.002 inches thick Ta foil, contains a Ta foil with TaO coating.
See John's Ipad for their recipes.
Evaporator #2 is now auto-ramping overnight at 0.2 A/min, up to 830 A, with the maximum voltage limited at 14 V, between 2.00e-05 (Good vacuum) and 3.00e-05 Torr (Bad vacuum).
|
Saturday, August 11, 2012, 19:15
Heating process was going smoothly up to 400 A. See Attachment 1.
Around 420 A, vacuum went up again and the voltage increased more quickly. It seems like resistance is building up. After reaching 530 A, the current was tapped down to 420 A in an effort to save the Ta boat. See Attachment 2.
The current will stay at 420 A for the weekend until John takes a look at this.
|
Monday, August 13, 2012, 13:46
TGHT was ramped down at 2 A/min and then tapped down to 0A. See Attachment 1. The target boat will be cooled down for about an hour before turning off the chiller.
|
Tuesday, August 14, 2012, 16:56
Summary:
The purpose of this experiment is to test the chemical and high temperature (1600C) resistance of a Ta foil (0.001" thick) coated with Ta2O5, so it can be used as the under-layer for the BeO sintering process.
The Ta2O5 (white powder, -325 mesh) was prepared in a non-aqueous solution and was sprayed on a piece of Ta foil.
The coated foil was rolled up and inserted in a Ta-coated (previously sintered) target boat for heating.
The foil was heated up to 520A (~1200C) and evidently,Ta2O5 started to react with Ta foil, and the foil became brittle and cracked (see attachment#1).
In conclusion, Ta2O5 is not a good protection layer for Ta material - at least for our applications.
|
Tuesday, August 14, 2012, 15:57, John Wong, SiC, 38295-8 , HP-FEBIAD, Done, Testing endcaps inserted /w the new expansion tool
|
Tuesday, August 14, 2012, 15:44
This SiC target was prepared in May 2011 with the Evaporator#1. The target will not used for online.
Two endcaps were inserted with the new expansion tool. The target will be heated up to the normal operating condition (TGHT =580A, TBHT = 230A).
The chamber is currently being pumped down.
Tuesday, August 14, 2012, 16:21
Earlier, the Cu-heat shield was removed from the evaporator to replace the insulators, so all the seals were placed with new ones. However,
there seems to be some leaks after the HS cooling water is turned on. (see attachment#1).
The TP off, and the chamber is vented for investigation.
Tuesday, August 14, 2012, 17:25
All the 3 seals for the Cu-heat shield were replaced. The chamber has been pumped down and the HS water valve is open. No leaks are detected.
Tuesday, August 14, 2012, 17:29
Initiated auto-ramping at 2A/min for both TGHT and TBHT.
Parameter constraints: good vac @ 2.0e-5 Torr, bad vac @ 3.0e-5 Torr.
Currently, IG1 @ 6.5e-6 Torr.
Wednesday, August 15, 2012, 09:52
TGHT and TBHT have reached to 520A and 230A, respectively, and have stayed at the currents for about 10 hours. (see attachment #2)
IG is currently at 7.7e-7 Torr.
Initiating auto-cool down at 2A/min.
Thursday, August 16, 2012, 11:23
Chamber is vented.
|
Tuesday, August 14, 2012, 15:11, John Wong, , , , Maintenance, Replacing Cu-heatshield insulators
|
Tuesday, August 14, 2012, 15:01
The Cu-heatshield insulators are broken due to prolong heating time during the target processes (see attachment#1).
The insulators are replaced with the MM800 type (see attachment #2).
|
Monday, July 30, 2012, 15:42, John Wong, , , , Problems, Chiller maybe leaky
|
Monday, July 30, 2012, 15:38
The evaporator was used for the processing the NiO target for 8 days and it was discovered today that there was a puddle of water underneath the chiller.
The cover of the chiller was removed and some water around the plumbing was found (see attachment #1).
Will continue to keep running the chiller to see if there is more water leaking out...
|
Sunday, July 22, 2012, 20:51, John Wong, NiO, 38481-7, HP-FEBIAD, Done, Sintering NiO#1
|
Sunday, July 22, 2012, 20:30
The NiO target materials were loaded into the container today.
Total discs = 500, (10 discs/pack)
length (after loaded) = 9.0cm
Target container is wrapped with Ta-heat shields, and will be removed after the sintering process.
One regular end cap is inserted (with Ni-foil inserted as a divider). The caps, however, are very loose (tried 2 caps and still loose). Hopefully the thermo diffusion bonding will seal the cap...
The other end is inserted with a D-cap for out-gassing proposes, and will be replaced with the regular end-cap after the process.
(see attachment#1)
Sunday, July 22, 2012, 20:48
The camber has been pumped down and currently IG1=1.3e-6 Torr.
The HS cooling water was turned on and no leaks were detected.
TGHT and TBHT were stepped up to 50A.
Auto-ramping is initiated at 0.2A/min for TGHT max = 250A, TBHT max = 230A.
Thursday, July 26, 2012, 23:31
TGHT and TBHT have reached to 250A (local @ 242A/2.88V) and 230A, respectively, and have stayed for ~4hrs (see attachment#2)
Currently, IGP1 = 4.9e-7 Torr, IGP2 = 3.5e-7 Torr, CG1B = 13mTorr.
Initiating auto-cool down at 2A/min.
Monday, July 30, 2012, 15:11
The chamber was vented and the target was removed.
There was significant condensation oily fluid coated Cu-heatshield lid and around the ionizer opening.
Overall, the target looks very good. The NiO target material was nicely sintered. No shrinkage or loose particles were observed (see attachment #3).
The endcap, however, was not properly fitted and it just fell off, (see attachment #4).
Both ends of the target are currently opened; the expension tool for the endcap is in order and hopefully this will solve the problem.
The target is being stored in the fumehood
|
Thursday, July 19, 2012, 17:05, John Wong, Empty, 37918-3, LP-FEBIAD, Done, Coating target oven /w TaC & sintering for UCx#5
|
Thursday, July 19, 2012, 16:58
The target container was coated with TaC.
It's wrapped with 3 layers of Ta as the heat-shield, including the backblock.
TGHT will be ramped up to 580A at 0.2A/min.
TBHT will be ramped up to 230A at 0.2A/min.
Currently, IGP1 = 1.5e-6 Torr. BP = 15mTorr
Friday, July 20, 2012, 13:56
TGHT and TBHT reached to 580A & 230A, respectively, and stayed for ~ 2hrs.
Measured temperature at the ionizer tube to be 1630C.
Cooling down in process at 2A/min...
Sunday, July 22, 2012, 20:53
The chamber was vented earlier around 14:00hr.
The target container looks good!
|
Tuesday, July 17, 2012, 16:00, John Wong, , targetboat (TaC coated), , Done, Sintering TaC coated regular- & D-endcaps
|
Tuesday, July 17, 2012, 15:45
Target boat is filled with TaC coated regular- and D-endcaps.
The boat is wrapped with a Ta heat-shield.
Chamber is being pumped down, currently at 5e-6 Torr.
Tuesday, July 17, 2012, 15:58
Heat-shield cooling water valve opened; no leaks detected.
Initiated TGHT auto-ramping at 0.5A/min, set TGHT max at 580A.
Wednesday, July 18, 2012, 10:44
Yesterday evening, the target heater tripped off a few times due to high vacuum excursion. The TGHT ramping rate was low to 0.2A/min. The current was ramped up sturdily to 500A this morning.
Wednesday, July 18, 2012, 10:46
Increased ramping rate to 2A/min. Vacuum currently at 2.2e-6 Torr.
Wednesday, July 18, 2012, 16:18
TGHt has reached to 580A and stayed for about 5 hrs.
Cooling down in process... 2A/min for TGHT --> 0A.
Thursday, July 19, 2012, 10:31
TGHT reached to 0A.
Evaporator is off.
Venting chamber...
|
Thursday, July 12, 2012, 17:55, John Wong, NiO, targetboat (TaC coated), , Maintenance, NiO development- test#2
|
Thursday, July 12, 2012, 17:29
NiO was sprayed on Ni foil.
Average/discs: mass= 0.075g, thickness=0.076mm, density = 7.023g/cm3.
4 set of samples were loaded onto the targetboat (coated/sintered with TaC). A piece of Ta foil was used as the under layer (see attachment #1).
A 0.002" thick Ta foil was wrapped around the container as the heat-shield.
The chamber was pumped down to 5.0e-6 Torr before the cooling water valve was opened; no leaks was detected.
For this process, the target heater will only go up to 250A (~1100C), with auto-ramping rate at 0.5A/min.
The heater has been stepped up to 50A, local 32A/ 0.23V. The vacuum reached to max 1.6e-5 Torr, and it's coming down.
Thursday, July 12, 2012, 17:51
Auto-ramping initiated...
Friday, July 13, 2012, 09:42
TGHT reached to 250A and stayed for 6 hrs (see attachment #2). At that current, the target wasn't glowing so the temperature could not be measured.
Initiated auto-cooling at 2A/min.
Friday, July 13, 2012, 11:00
TGHT reached to 65A. Stopped the auto-cooling process and manually tapped down the p/s to 0A.
Vacuum is stable at 5.7e-7 Torr.
In the next 30 min or so, the chamber will be vented and the NiO target material will be taken out for inspection.
|
Wednesday, June 20, 2012, 17:29, Nikita Bernier, NiO, Ta target boat, , Done, NiO development
|
Wednesday, June 20, 2012, 17:23
New Target boat, with no coating, wrapped with a 0.002 inches thick Ta foil, contains 3 NiO pellets :
Sample, # Disks, Mass (g), Thickness (mm)
1 12, 1.9396, 1.938
2 13, 0.9592, 0.847
3 25, 2.6675, 3.06
See John's Ipad for their recipes.
Evaporator #2 is now auto-ramping overnight at 0.5 A/min, up to 580 A, with the maximum voltage limited at 14 V, between 3.00e-05 (Good vacuum) and 4.00e-05 Torr (Bad vacuum).
Thursday, June 21, 2012, 18:14
See attachment #1, 2 for the density measurements and the graph for the disc thickness -JW
|
Wednesday, June 20, 2012, 22:33, John Wong, NiO, Ta target boat, , Done, NiO development
|
Nikita Bernier wrote: |
Wednesday, June 20, 2012, 17:23
New Target boat, with no coating, wrapped with a 0.002 inches thick Ta foil, contains NiO D-shape discs :
Sample, # Disks, Mass (g), Thickness (mm)
1 12, 1.9396, 1.938
2 13, 0.9592, 0.847
3 25, 2.6675, 3.06
See John's Ipad for their recipes.
Evaporator #2 is now auto-ramping overnight at 0.5 A/min, up to 580 A, with the maximum voltage limited at 14 V, between 3.00e-05 (Good vacuum) and 4.00e-05 Torr (Bad vacuum).
|
Wednesday, June 20, 2012, 22:28
TGHT tripped off at 78A due to high out-gassing pressure. The current was tapped down to 75A before it was turned back on.
Changed ramping rate from 0.5A/min to 0.2A/min.
Initiate auto-ramping...
Thursday, June 21, 2012, 08:35
Vacuum has come down to 7e-7 as TGHT is being ramped up at 0.2A/min. (see attachment#1).
Increase TGHT rate to 2A/min.
The temperature should be measured when the heater gets up to around 500A.
|
Thursday, June 21, 2012, 18:13, John Wong, NiO, Ta target boat, , Failed, NiO development - Container broke!
|
John Wong wrote: |
Nikita Bernier wrote: |
Wednesday, June 20, 2012, 17:23
New Target boat, with no coating, wrapped with a 0.002 inches thick Ta foil, contains NiO D-shape discs :
Sample, # Disks, Mass (g), Thickness (mm)
1 12, 1.9396, 1.938
2 13, 0.9592, 0.847
3 25, 2.6675, 3.06
See John's Ipad for their recipes.
Evaporator #2 is now auto-ramping overnight at 0.5 A/min, up to 580 A, with the maximum voltage limited at 14 V, between 3.00e-05 (Good vacuum) and 4.00e-05 Torr (Bad vacuum).
|
Wednesday, June 20, 2012, 22:28
TGHT tripped off at 78A due to high out-gassing pressure. The current was tapped down to 75A before it was turned back on.
Changed ramping rate from 0.5A/min to 0.2A/min.
Initiate auto-ramping...
Thursday, June 21, 2012, 08:35
Vacuum has come down to 7e-7 as TGHT is being ramped up at 0.2A/min. (see attachment#1).
Increase TGHT rate to 2A/min.
The temperature should be measured when the heater gets up to around 500A.
|
Thursday, June 21, 2012, 17:37
The NiO discs were heated up to 1500C at 560A. The target heater was lowered in steps and the temperature was measured. At 320A, the target container was ~1110C. (see attachment #1)
There was a sign of resistant on the target container as the p/s voltage started to go up at a higher rate. (see attachment#2, 3, 4 for the archived striptool).
Unfortunately, the target container was broken; it was most likely reacted with the Ni. (see attachment#5)
So.... the possible solution?! TRY coating the container with Ta2O5. Will discuss more in the Friday Jun 22 meeting.
|
Tuesday, May 15, 2012, 12:26, John Wong, SiC, 38481-2, HP-SIS, Done, Re-condition the HP-SIS SiC target
|
Tuesday, May 15, 2012, 12:24
The HP-SIS SiC target was made on Nov 03, 2010. The target consists of 405 discs, 18.5cm in length. It was sintered in the Evaporator#1.
This target is going into Evap#2 for re-conditioning. It is currently being pumped down.
|
Friday, May 18, 2012, 12:19, Nikita Bernier, SiC, 38481-2, HP-SIS, Done, Re-condition the HP-SIS SiC target
|
John Wong wrote: |
Tuesday, May 15, 2012, 12:24
The HP-SIS SiC target was made on Nov 03, 2010. The target consists of 405 discs, 18.5cm in length. It was sintered in the Evaporator#1.
This target is going into Evap#2 for re-conditioning. It is currently being pumped down.
|
Friday, May 18, 2012, 12:19
The target is wrapped with only one heat shield.
Evaporator #2 Target Heater is now auto-ramping at 0.5 A/min, up to 820 A, with the maximum voltage limited at 2 V, between 2.00e-05 (Good vacuum) and 3.00e-05 Torr (Bad vacuum). Tube Heater is auto-ramping at 0.5 A/min, up to 230 A, with the maximum voltage limited at 1 V. See attachments.
|
Friday, May 18, 2012, 13:17, John Wong, SiC, 38481-2, HP-SIS, Done, Re-condition the HP-SIS SiC target
|
Nikita Bernier wrote: |
John Wong wrote: |
Tuesday, May 15, 2012, 12:24
The HP-SIS SiC target was made on Nov 03, 2010. The target consists of 405 discs, 18.5cm in length. It was sintered in the Evaporator#1.
This target is going into Evap#2 for re-conditioning. It is currently being pumped down.
|
Friday, May 18, 2012, 12:19
The target is wrapped with only one heat shield.
Evaporator #2 Target Heater is now auto-ramping at 0.5 A/min, up to 820 A, with the maximum voltage limited at 2 V, between 2.00e-05 (Good vacuum) and 3.00e-05 Torr (Bad vacuum). Tube Heater is auto-ramping at 0.5 A/min, up to 230 A, with the maximum voltage limited at 1 V. See attachments.
|
Friday, May 18, 2012, 13:15
Increased TBHT voltage to 5V, and TGHT to 15V. Currently, TBHT =83A, 0.986V, TGHT= 144A, 1.65V, IGP1 = 5.2e-7 Torr, IGP2 = 4.3e-7 Torr.
Continue ramping up...
Tuesday, May 22, 2012, 12:02
TGHT and TBHT were ramped up to 830A/13.65V (local), and 235A/3.85V, respectively. The target was conditioned over the long weekend.
|
Tuesday, May 22, 2012, 12:15, Nikita Bernier, SiC, 38481-2, HP-SIS, Done, Re-condition the HP-SIS SiC target
|
John Wong wrote: |
Nikita Bernier wrote: |
John Wong wrote: |
Tuesday, May 15, 2012, 12:24
The HP-SIS SiC target was made on Nov 03, 2010. The target consists of 405 discs, 18.5cm in length. It was sintered in the Evaporator#1.
This target is going into Evap#2 for re-conditioning. It is currently being pumped down.
|
Friday, May 18, 2012, 12:19
The target is wrapped with only one heat shield.
Evaporator #2 Target Heater is now auto-ramping at 0.5 A/min, up to 820 A, with the maximum voltage limited at 2 V, between 2.00e-05 (Good vacuum) and 3.00e-05 Torr (Bad vacuum). Tube Heater is auto-ramping at 0.5 A/min, up to 230 A, with the maximum voltage limited at 1 V. See attachments.
|
Friday, May 18, 2012, 13:15
Increased TBHT voltage to 5V, and TGHT to 15V. Currently, TBHT =83A, 0.986V, TGHT= 144A, 1.65V, IGP1 = 5.2e-7 Torr, IGP2 = 4.3e-7 Torr.
Continue ramping up...
Tuesday, May 22, 2012, 12:02
TGHT and TBHT were ramped up to 830A/13.65V (local), and 235A/3.85V, respectively. The target was conditioned over the long weekend.
|
Tuesday, May 22, 2012, 12:13
Initiating the cool-down process at 5 A/min.
See archive plots of the Target Heater (Attachment 1) and the Tube Heater (Attachment 2). |
Tuesday, May 22, 2012, 15:26, John Wong, SiC, 38481-2, HP-SIS, Done, Re-condition the HP-SIS SiC target
|
Nikita Bernier wrote: |
John Wong wrote: |
Nikita Bernier wrote: |
John Wong wrote: |
Tuesday, May 15, 2012, 12:24
The HP-SIS SiC target was made on Nov 03, 2010. The target consists of 405 discs, 18.5cm in length. It was sintered in the Evaporator#1.
This target is going into Evap#2 for re-conditioning. It is currently being pumped down.
|
Friday, May 18, 2012, 12:19
The target is wrapped with only one heat shield.
Evaporator #2 Target Heater is now auto-ramping at 0.5 A/min, up to 820 A, with the maximum voltage limited at 2 V, between 2.00e-05 (Good vacuum) and 3.00e-05 Torr (Bad vacuum). Tube Heater is auto-ramping at 0.5 A/min, up to 230 A, with the maximum voltage limited at 1 V. See attachments.
|
Friday, May 18, 2012, 13:15
Increased TBHT voltage to 5V, and TGHT to 15V. Currently, TBHT =83A, 0.986V, TGHT= 144A, 1.65V, IGP1 = 5.2e-7 Torr, IGP2 = 4.3e-7 Torr.
Continue ramping up...
Tuesday, May 22, 2012, 12:02
TGHT and TBHT were ramped up to 830A/13.65V (local), and 235A/3.85V, respectively. The target was conditioned over the long weekend.
|
Tuesday, May 22, 2012, 12:13
Initiating the cool-down process at 5 A/min.
See archive plots of the Target Heater (Attachment 1) and the Tube Heater (Attachment 2).
|
Tuesday, May 22, 2012, 15:24
TGHT/TBHT were ramped down to 0A. The target has cooled for about 45 min. All pumps and chillers are off. The chamber has been vented.
|
Monday, June 11, 2012, 12:26, John Wong, SiC, 38481-2, HP-SIS, Problems, End caps vaporized
|
John Wong wrote: |
Nikita Bernier wrote: |
John Wong wrote: |
Nikita Bernier wrote: |
John Wong wrote: |
Tuesday, May 15, 2012, 12:24
The HP-SIS SiC target was made on Nov 03, 2010. The target consists of 405 discs, 18.5cm in length. It was sintered in the Evaporator#1.
This target is going into Evap#2 for re-conditioning. It is currently being pumped down.
|
Friday, May 18, 2012, 12:19
The target is wrapped with only one heat shield.
Evaporator #2 Target Heater is now auto-ramping at 0.5 A/min, up to 820 A, with the maximum voltage limited at 2 V, between 2.00e-05 (Good vacuum) and 3.00e-05 Torr (Bad vacuum). Tube Heater is auto-ramping at 0.5 A/min, up to 230 A, with the maximum voltage limited at 1 V. See attachments.
|
Friday, May 18, 2012, 13:15
Increased TBHT voltage to 5V, and TGHT to 15V. Currently, TBHT =83A, 0.986V, TGHT= 144A, 1.65V, IGP1 = 5.2e-7 Torr, IGP2 = 4.3e-7 Torr.
Continue ramping up...
Tuesday, May 22, 2012, 12:02
TGHT and TBHT were ramped up to 830A/13.65V (local), and 235A/3.85V, respectively. The target was conditioned over the long weekend.
|
Tuesday, May 22, 2012, 12:13
Initiating the cool-down process at 5 A/min.
See archive plots of the Target Heater (Attachment 1) and the Tube Heater (Attachment 2).
|
Tuesday, May 22, 2012, 15:24
TGHT/TBHT were ramped down to 0A. The target has cooled for about 45 min. All pumps and chillers are off. The chamber has been vented.
|
Monday, June 11, 2012, 12:20
After the re-conditioning, the target's end-caps vaporized. This is something happened before (see elog entries below):
https://elog.triumf.ca/TIS/Evaporator_1/20
https://elog.triumf.ca/TIS/Evaporator_1/22
The caps were removed and yellow crystals were observed. (see attachment#1).
The D-caps will be inserted in both ends and will be re-conditioned again to see if the yellow crystals can be removed at high temperature.
|
Thursday, April 05, 2012, 16:40, Nikita Bernier, BeO, Target boat #2, , Done, Sintering BeO pellets #3
|
Thursday, April 05, 2012, 16:31
Target boat contains 6 BeO pellets :
Sample, Mass (g), Thickness (mm), Density (g/cm3)
1 1.2842, 5.406, 1.4647
2 1.2619, 5.150, 1.5108
3 1.2886, 5.316, 1.4946
4 1.2858, 5.310, 1.4931
5 1.3382, 5.520, 1.4948
6 1.3916, 5.650, 1.5187
Samples are made of BeO powder with 30% PVB which was treated at 400 RPM for 26 minutes. A ratio of 1:0.1 of mineral oil was added before another high speed treatment for 10 minutes. The powder was then pressed into pellets.
Pellets are loaded on a target boat coated/sintered with TaC. The target boat is wrapped with a Ta foil that is 0.002 inches thick.
**** Sintering is postponed until the situation with the ventilation in the lab06 is cleared. ****
|
Tuesday, May 22, 2012, 16:45, Nikita Bernier, BeO, Target boat #2, , Done, Sintering BeO pellets #3
|
Nikita Bernier wrote: |
Thursday, April 05, 2012, 16:31
Target boat contains 6 BeO pellets :
Sample, Mass (g), Thickness (mm), Density (g/cm3)
1 1.2842, 5.406, 1.4647
2 1.2619, 5.150, 1.5108
3 1.2886, 5.316, 1.4946
4 1.2858, 5.310, 1.4931
5 1.3382, 5.520, 1.4948
6 1.3916, 5.650, 1.5187
Samples are made of BeO powder with 30% PVB which was treated at 400 RPM for 26 minutes. A ratio of 1:0.1 of mineral oil was added before another high speed treatment for 10 minutes. The powder was then pressed into pellets.
Pellets are loaded on a target boat coated/sintered with TaC. The target boat is wrapped with a Ta foil that is 0.002 inches thick.
**** Sintering is postponed until the situation with the ventilation in the lab06 is cleared. ****
|
Tuesday, May 22, 2012, 16:44
Target chamber is currently being pumped down. Leak check will be done tomorrow by turning on the cooling water for the heat shield. |
Wednesday, May 23, 2012, 17:45, John Wong, BeO, Target boat #2, , Done, Sintering BeO pellets #3
|
Nikita Bernier wrote: |
Nikita Bernier wrote: |
Thursday, April 05, 2012, 16:31
Target boat contains 6 BeO pellets :
Sample, Mass (g), Thickness (mm), Density (g/cm3)
1 1.2842, 5.406, 1.4647
2 1.2619, 5.150, 1.5108
3 1.2886, 5.316, 1.4946
4 1.2858, 5.310, 1.4931
5 1.3382, 5.520, 1.4948
6 1.3916, 5.650, 1.5187
Samples are made of BeO powder with 30% PVB which was treated at 400 RPM for 26 minutes. A ratio of 1:0.1 of mineral oil was added before another high speed treatment for 10 minutes. The powder was then pressed into pellets.
Pellets are loaded on a target boat coated/sintered with TaC. The target boat is wrapped with a Ta foil that is 0.002 inches thick.
**** Sintering is postponed until the situation with the ventilation in the lab06 is cleared. ****
|
Tuesday, May 22, 2012, 16:44
Target chamber is currently being pumped down. Leak check will be done tomorrow by turning on the cooling water for the heat shield.
|
Wednesday, May 23, 2012, 17:38
TGHT was stepped up to about 55A before the auto ramping was initiated. The vacuum limit parameter was set for good vac at <4.0 e-5 Torr and bad vac at >5.0 e0-5 Torr.
The pressure is coming close to the trip limit (8.5 e-5 Torr) (see attachment 1: strip tool over the past 5 hours). Changed the vacuum limit parameter: good vac =3.0e-5 Torr, bad vac= 4.0e-5 Torr.
Saturday, May 26, 2012, 10:44
TGHT is auto ramping up smoothly as the pressure is regulating between 1e-5 to 4 e-5 torr. (See attachment 2, past 21 hr)
Sunday, May 27, 2012, 12:25
There could be a power bump early this morning at 06:30hr, and tripped off the TGHT power supply (see attachment #3). The computer in the cold lab was found to be off expectedly, so the alarm handler running on that computer was also shut off (*Need a UPS on this computer!)
Called the ISAC Ops, and nothing about any power bump around that time was noticed.
Turned on TGHT p/s and set TGHT at 318A, local at 315A/4.58V. TGHT has been running for about 10 mins. Currently vac at 4.2e-7 Torr.
Sunday, May 27, 2012, 12:35
Initiating TGHT auto ramping...
Monday, May 28, 2012, 00:20
TGHT has reached to 600A and will remain at that current for the rest of the night. The target oven temperature will be measured tomorrow.
See attachment#4 for the striptool over the past 10hr.
Monday, May 28, 2012, 10:56
TGHT stayed at 600A for about 12 hours. Pressure gradually came down to 7.6e-7 Torr. (See attachment #5).
At TGHT=600A, The target boat temperature was measured at 1400C (with the pyrometer), and the Ta-heat shield (1-layer) was at 1050C. [Note: These temperature measurements are very closed to the measurements with an empty LP target (with not heat shield), TGHT @ 600A = 1360C].
Monday, May 28, 2012, 11:04
Due to the water leak from the Evap2 chiller, the system has to be shut off for inspection.
TGHT was tapped down to 0A. The target was cooled down for about 20min before the chiller was turned off.
Will continue with the process after the problem is solved...
|
Tuesday, May 29, 2012, 15:43, Nikita Bernier, BeO, Target boat #2, , Failed, Sintering BeO pellets #3
|
John Wong wrote: |
Nikita Bernier wrote: |
Nikita Bernier wrote: |
Thursday, April 05, 2012, 16:31
Target boat contains 6 BeO pellets :
Sample, Mass (g), Thickness (mm), Density (g/cm3)
1 1.2842, 5.406, 1.4647
2 1.2619, 5.150, 1.5108
3 1.2886, 5.316, 1.4946
4 1.2858, 5.310, 1.4931
5 1.3382, 5.520, 1.4948
6 1.3916, 5.650, 1.5187
Samples are made of BeO powder with 30% PVB which was treated at 400 RPM for 26 minutes. A ratio of 1:0.1 of mineral oil was added before another high speed treatment for 10 minutes. The powder was then pressed into pellets.
Pellets are loaded on a target boat coated/sintered with TaC. The target boat is wrapped with a Ta foil that is 0.002 inches thick.
**** Sintering is postponed until the situation with the ventilation in the lab06 is cleared. ****
|
Tuesday, May 22, 2012, 16:44
Target chamber is currently being pumped down. Leak check will be done tomorrow by turning on the cooling water for the heat shield.
|
Wednesday, May 23, 2012, 17:38
TGHT was stepped up to about 55A before the auto ramping was initiated. The vacuum limit parameter was set for good vac at <4.0 e-5 Torr and bad vac at >5.0 e0-5 Torr.
The pressure is coming close to the trip limit (8.5 e-5 Torr) (see attachment 1: strip tool over the past 5 hours). Changed the vacuum limit parameter: good vac =3.0e-5 Torr, bad vac= 4.0e-5 Torr.
Saturday, May 26, 2012, 10:44
TGHT is auto ramping up smoothly as the pressure is regulating between 1e-5 to 4 e-5 torr. (See attachment 2, past 21 hr)
Sunday, May 27, 2012, 12:25
There could be a power bump early this morning at 06:30hr, and tripped off the TGHT power supply (see attachment #3). The computer in the cold lab was found to be off expectedly, so the alarm handler running on that computer was also shut off (*Need a UPS on this computer!)
Called the ISAC Ops, and nothing about any power bump around that time was noticed.
Turned on TGHT p/s and set TGHT at 318A, local at 315A/4.58V. TGHT has been running for about 10 mins. Currently vac at 4.2e-7 Torr.
Sunday, May 27, 2012, 12:35
Initiating TGHT auto ramping...
Monday, May 28, 2012, 00:20
TGHT has reached to 600A and will remain at that current for the rest of the night. The target oven temperature will be measured tomorrow.
See attachment#4 for the striptool over the past 10hr.
Monday, May 28, 2012, 10:56
TGHT stayed at 600A for about 12 hours. Pressure gradually came down to 7.6e-7 Torr. (See attachment #5).
At TGHT=600A, The target boat temperature was measured at 1400C (with the pyrometer), and the Ta-heat shield (1-layer) was at 1050C. [Note: These temperature measurements are very closed to the measurements with an empty LP target (with not heat shield), TGHT @ 600A = 1360C].
Monday, May 28, 2012, 11:04
Due to the water leak from the Evap2 chiller, the system has to be shut off for inspection.
TGHT was tapped down to 0A. The target was cooled down for about 20min before the chiller was turned off.
Will continue with the process after the problem is solved...
|
Tuesday, May 29, 2012, 15:30
Evap2 was vented out and the pellets were taken out of the boat and examined.
The six pellets are cracked and have a greyish colour. The cracking is probably caused by the instant cooling and reheating when the system tripped on Sunday morning.
The light grey colour and white spots suggest that the sintering process was not completed and so the shrinkage cannot be determined.
A new batch of BeO pellets will have to be prepared and sintered in order to determine the dimensions of the final die.
|
Monday, May 28, 2012, 11:15, John Wong, , , , Problems, Chiller is leaking water
|
Monday, May 28, 2012, 11:08
It was discovered this morning that the Evaporator #2 chiller was leaking water from the bottom (see attachment 1). A puddle of water was formed and eventually found its way down to the Hotcell.
The evaporator was running over the weekend for the BeO pellets process. The TGHT is now off and the chiller will be inspected...
|
Tuesday, May 15, 2012, 17:03, John Wong, , , , Problems, TBHT cooling line leaky
|
Tuesday, May 15, 2012, 17:00
It was found that there were water droplets from the TBHT cooling line. The joint is leaky. (see attachment 1)
A message has sent to Rick M.
|
Wednesday, May 16, 2012, 14:04, John Wong, , , , Problems resolved, TBHT cooling line leaky
|
John Wong wrote: |
Tuesday, May 15, 2012, 17:00
It was found that there were water droplets from the TBHT cooling line. The joint is leaky. (see attachment 1)
A message has sent to Rick M.
|
Wednesday, May 16, 2012, 14:01
The connector was re-tighten. The water valve was opened, and no water leaks were found.
|
Tuesday, May 15, 2012, 17:06, John Wong, , , , Problems resolved, TBHT power supply faulty
|
Tuesday, May 15, 2012, 17:03
The tube heater power supply current readback and setpoint are not matching. Ray Dube checked the power supply and confirmed that it is faulty. He will replace a functional p/s tomorrow.
Friday, May 18, 2012, 13:24
The original p/s was replaced with a new one and there was still a discrepancy between the readback and the setpoint. After checking with the drawings for the ITE/ITW tube heaters, it was confirmed that the connections for the Evap#2 tube heater control were wrong. (see attachment 1). The connections were corrected and the power supply is now operational.
|
Tuesday, May 15, 2012, 14:00, John Wong, , , , Maintenance, Installed a new stainless metal heat shield
|
Tuesday, May 15, 2012, 13:45
It was discovered that one of the insulators that supported the target module broke apart (see Attachment#1). This might be caused by the heat from the target legs that reflected back from the base to the insulators. The burnt marks are the evidence.
A stainless metal sheet is used as the heat shield (see Attachment #2).
|
Tuesday, April 03, 2012, 09:00, John Wong, Empty, Ta-target boat #2, , , Sintering Ta-target boat with TaC coating
|
Tuesday, April 03, 2012, 08:54
Yesterday, a new target boat was sprayed with TaC coating and let dried.
The boat was then installed in the Evap#2 chamber and pumped down to 10-6 Torr before the target heater was turned on. NOTE: Target boat is not wrapped with Ta-heat shield.
TGHT auto ramping was initiated at 2.0A/min and max setpoint to 700A. The voltage was set at 3V; therefore, the current only ramped up to 250A over night.
--> Increased the TGHT voltage to 15A, and continue ramping the TGHT to 700A. Currently vac at low 2.3e-7 Torr.
Tuesday, April 03, 2012, 09:12
The vac is at low 10e-7 as the TGHT is ramping up. Changing ramping rate from 2A/min to 5A/min.
Tuesday, April 03, 2012, 12:00
TGHT reached to 700A. Measured temp @ 1280C.
Tapped up TGHT to:
800A. Measured temp @ 1400C.
850A (local 843A/15.60V). Measured temp @ 1450C.
900A (local 893A/16.88V). Measured temp @ 1500C
Tuesday, April 03, 2012, 14:35:
Try autoramping TGHT to 1000A but voltage has gone up close to the max limit (20V). TGHT could only go up to ~970A (see attachment 1: TGHT_maxcurrent.jpg). The heater remained at that current for ~1hr but auto cooling was initiated - at 10A/min.
|
Thursday, March 29, 2012, 19:30, Nikita Bernier, BeO, Target boat #1, , Done, Sintering new BeO pellets
|
Thursday, March 29, 2012, 19:17
Target boat contains 3 BeO pellets :
Sample, Thickness (mm), Mass (g), Density (g/cm3)
1 9.06, 1.9713, 1.413
2 9.11, 1.9900, 1.419
3 13.54, 1.9916, 0.956
Samples 1 and 2 are made of BeO powder with 30% PVB which was washed with excess acetone and let to dry on a greased baking sheet (with PAM Butter flavoured). The flakes were then milled for 26 minutes at 400 RPM. It resulted in a very fine grey powder, much denser than the BeO powder with 30% PVB (not washed with acetone) that was used for Sample 3.
The initial settings on Evaporator #2 were 100 A and 0.83 V until the vacuum increased.
Evaporator #2 is now auto-ramping overnight at 1 A/min, up to 700 A, with the maximum voltage limited at 14 V, between 5.00e-05 (Good vacuum) and 6.00e-05 Torr (Bad vacuum).
|
Thursday, March 29, 2012, 22:44, John Wong, BeO, Target boat #1, , Done, Sintering new BeO pellets
|
Nikita Bernier wrote: |
Thursday, March 29, 2012, 19:17
Target boat contains 3 BeO pellets :
Sample, Thickness (mm), Mass (g), Density (g/cm3)
1 9.06, 1.9713, 1.413
2 9.11, 1.9900, 1.416
3 13.54, 1.9916, 0.956
Samples 1 and 2 are made of BeO powder with 30% PVB which was washed with excess acetone and let to dry on a greased baking sheet (with PAM Butter flavoured). The flakes were then milled for 26 minutes at 400 RPM. It resulted in a very fine grey powder, much denser than the BeO powder with 30% PVB (not washed with acetone) that was used for Sample 3.
The initial settings on Evaporator #2 were 100 A and 0.83 V until the vacuum increased.
Evaporator #2 is now auto-ramping overnight at 1 A/min, up to 700 A, with the maximum voltage limited at 14 V, between 5.00e-05 (Good vacuum) and 6.00e-05 Torr (Bad vacuum).
|
Thursday, March 29, 2012, 22:31:
TGHT tripped off a few times over the past hours. After changing the Good Vac to 2.00e-5 torr and Bad Vac to 3.00e-5 Torr, the target heater are regulating properly and the max pressure is well maintained below 6.5e-5 Torr [Trip point @ 8.0e-5 Torr]. (see attachment#1: parameter.jpg) |
Friday, March 30, 2012, 23:21, John Wong, BeO, Target boat #1, , Done, Sintering new BeO pellets
|
John Wong wrote: |
Nikita Bernier wrote: |
Thursday, March 29, 2012, 19:17
Target boat contains 3 BeO pellets :
Sample, Thickness (mm), Mass (g), Density (g/cm3)
1 9.06, 1.9713, 1.413
2 9.11, 1.9900, 1.416
3 13.54, 1.9916, 0.956
Samples 1 and 2 are made of BeO powder with 30% PVB which was washed with excess acetone and let to dry on a greased baking sheet (with PAM Butter flavoured). The flakes were then milled for 26 minutes at 400 RPM. It resulted in a very fine grey powder, much denser than the BeO powder with 30% PVB (not washed with acetone) that was used for Sample 3.
The initial settings on Evaporator #2 were 100 A and 0.83 V until the vacuum increased.
Evaporator #2 is now auto-ramping overnight at 1 A/min, up to 700 A, with the maximum voltage limited at 14 V, between 5.00e-05 (Good vacuum) and 6.00e-05 Torr (Bad vacuum).
|
Thursday, March 29, 2012, 22:31:
TGHT tripped off a few times over the past hours. After changing the Good Vac to 2.00e-5 torr and Bad Vac to 3.00e-5 Torr, the target heater are regulating properly and the max pressure is well maintained below 6.5e-5 Torr [Trip point @ 8.0e-5 Torr]. (see attachment#1: parameter.jpg)
|
Friday, March 30, 2012, 23:19
Archive of the target current and vacuum over the past 24 hours. (see attachment #1: archive_24hr)
Saturday, March 31, 2012, 12:12
The organic materials have been burnt off. The target heater ramping up is no longer restricted by the vacuum limit.
Archive of the target current and vacuum over the past 10 hours. (see attachment #2: TGHT@240A).
Saturday, March 31, 2012, 22:52
TGHT has stayed at 700A/12.37V, local @ 693A/12.43 = Temp @ 1780C.
The striptool shows some out-gassing when TGHT reached to 700A. (see attachment #3 marked with black circle: TGHT@700A.jpg)
Increasing TGHT to 750A to see if there is any further reaction...
Sunday, April 01, 2012, 10:24
TGHT was ramped up to 750A, local 730A/13.90V. The pressure has come down to low 10e-6 but not stable; Some reaction may be ongoing therefore it's causing the vacuum excursion. (See attachment #4: TGHT @ 750A). Notice the current readback is not constant and it's slowly decreasing as the voltage readback is increasing. There might be some resistant building up.
--> Initiating the cool-down process at 2A/min.
Sunday, April 01, 2012, 19:30
TGHT has ramped down to 0A, and the pressure is going down (currently at 7.e-8 Torr) with no excursion. (see attachment #5: TGHT@0A).
The chamber will be vented tomorrow, and the target materials will be inspected.
|
Monday, April 02, 2012, 16:26, Nikita Bernier, BeO, Target boat #1, , Done, Sintering new BeO pellets
|
John Wong wrote: |
John Wong wrote: |
Nikita Bernier wrote: |
Thursday, March 29, 2012, 19:17
Target boat contains 3 BeO pellets :
Sample, Thickness (mm), Mass (g), Density (g/cm3)
1 9.06, 1.9713, 1.413
2 9.11, 1.9900, 1.416
3 13.54, 1.9916, 0.956
Samples 1 and 2 are made of BeO powder with 30% PVB which was washed with excess acetone and let to dry on a greased baking sheet (with PAM Butter flavoured). The flakes were then milled for 26 minutes at 400 RPM. It resulted in a very fine grey powder, much denser than the BeO powder with 30% PVB (not washed with acetone) that was used for Sample 3.
The initial settings on Evaporator #2 were 100 A and 0.83 V until the vacuum increased.
Evaporator #2 is now auto-ramping overnight at 1 A/min, up to 700 A, with the maximum voltage limited at 14 V, between 5.00e-05 (Good vacuum) and 6.00e-05 Torr (Bad vacuum).
|
Thursday, March 29, 2012, 22:31:
TGHT tripped off a few times over the past hours. After changing the Good Vac to 2.00e-5 torr and Bad Vac to 3.00e-5 Torr, the target heater are regulating properly and the max pressure is well maintained below 6.5e-5 Torr [Trip point @ 8.0e-5 Torr]. (see attachment#1: parameter.jpg)
|
Friday, March 30, 2012, 23:19
Archive of the target current and vacuum over the past 24 hours. (see attachment #1: archive_24hr)
Saturday, March 31, 2012, 12:12
The organic materials have been burnt off. The target heater ramping up is no longer restricted by the vacuum limit.
Archive of the target current and vacuum over the past 10 hours. (see attachment #2: TGHT@240A).
Saturday, March 31, 2012, 22:52
TGHT has stayed at 700A/12.37V, local @ 693A/12.43 = Temp @ 1780C.
The striptool shows some out-gassing when TGHT reached to 700A. (see attachment #3 marked with black circle: TGHT@700A.jpg)
Increasing TGHT to 750A to see if there is any further reaction...
Sunday, April 01, 2012, 10:24
TGHT was ramped up to 750A, local 730A/13.90V. The pressure has come down to low 10e-6 but not stable; Some reaction may be ongoing therefore it's causing the vacuum excursion. (See attachment #4: TGHT @ 750A). Notice the current readback is not constant and it's slowly decreasing as the voltage readback is increasing. There might be some resistant building up.
--> Initiating the cool-down process at 2A/min.
Sunday, April 01, 2012, 19:30
TGHT has ramped down to 0A, and the pressure is going down (currently at 7.e-8 Torr) with no excursion. (see attachment #5: TGHT@0A).
The chamber will be vented tomorrow, and the target materials will be inspected.
|
Monday, April 02, 2012, 16:11
After sintering , the 3 BeO pellets have shrunk and feel robust.
The first sample ate through the Ta target boat, shrank a lot and has white and black marks. We suspect the PAM (mostly made of canola oil) to be responsible for the boat damage and the weird sintering process (see John's posts).
Sample 2 is holding well.
Sample 3, which was not washed with acetone, shows some cracks.
Sample, Thickness (mm), Mass (g), Density (g/cm3)
1 -----, 0.6254, -----
2 5.81, 0.9229, 1.032
3 8.89, 1.1073, 0.809
The average mass before sintering was 1.9843 g. After sintering, 0.8852 g. Thus the average mass loss is 0.9757 (49.0%).
We are starting a new batch of treated powder washed with acetone without PAM.
|
Monday, March 19, 2012, 17:10, Nikita Bernier, BeO, Target boat #1, , Done, Sintering BeO pellets
|
Monday, March 19, 2012, 17:04
Target boat contains 4 BeO pellets with 30% PVB:
Sample, Thickness (mm), Mass (g), Density (g/cm3)
1 4.943, 0.9628, 1.265
2 4.930, 0.9685, 1.276
3 4.758, 0.9607, 1.312
4 4.979, 0.9872, 1.288
Target chamber is currently being pumped down. Leak check will be done tomorrow by turning on the cooling water for the heat shield.
Wednesday, March 21, 2012, 18:30
The Evaporator #2 backing pump (IEVAP2BP1) muffler has been connected to the exhaust system.
The auto-ramp program has been tested today and works well.
Evaporator #2 is now auto-ramping overnight at 1 A/min, up to 500 A, between 5.00e-05 and 6.00e-05 Torr.
ISAC ops have been informed of the process and they will include it in their walkaround. |
Tuesday, March 20, 2012, 14:39, John Wong, BeO, Target boat #1, , Done, Sintering BeO pellets
|
Nikita Bernier wrote: |
Monday, March 19, 2012, 17:04
Target boat contains 4 BeO pellets with 30% PVB:
Sample, Thickness (mm), Mass (g), Density (g/cm3)
1 4.943, 0.9628, 1.265
2 4.930, 0.9685, 1.276
3 4.758, 0.9607, 1.312
4 4.979, 0.9872, 1.288
Target chamber is currently being pumped down. Leak check will be done tomorrow by turning on the cooling water for the heat shield.
|
Tuesday, March 20, 2012, 14:35
It was found out that the Evaporator #2 backing pump (IEVAP2BP1) muffler is not connected to the exhaust system. The sintering process is on hold until the pump is properly setup (see message ID#7 for more details).
|
Thursday, March 22, 2012, 00:34, John Wong, BeO, Target boat #1, , Done, Sintering BeO pellets
|
Nikita Bernier wrote: |
Monday, March 19, 2012, 17:04
Target boat contains 4 BeO pellets with 30% PVB:
Sample, Thickness (mm), Mass (g), Density (g/cm3)
1 4.943, 0.9628, 1.265
2 4.930, 0.9685, 1.276
3 4.758, 0.9607, 1.312
4 4.979, 0.9872, 1.288
Target chamber is currently being pumped down. Leak check will be done tomorrow by turning on the cooling water for the heat shield.
* Note: Target a boat is wrapped with a piece of Ta-foil as a heat shield - JW.
Wednesday, March 21, 2012, 18:30
The Evaporator #2 backing pump (IEVAP2BP1) muffler has been connected to the exhaust system.
The auto-ramp program has been tested today and works well.
Evaporator #2 is now auto-ramping overnight at 1 A/min, up to 500 A, between 5.00e-05 and 6.00e-05 Torr.
ISAC ops have been informed of the process and they will include it in their walkaround.
|
Thursday, March 22, 2012, 00:25
TGHT SETPOINT was ramped up to 266A but the actual p/s current remained at 90A; that was because the voltage was set 1.05V. (See attachment1: voltage_limiting.jpg).
Increased TGHT voltage to 20V, and increased the auto-ramping final value from 500A to 1000A (~1780C as previously measured by a pyrometer, see Attachment 2: Temp-Cal vs Measured.jgp)
Thursday, March 22, 2012, 10:17
TGHT ramped up at the rate of 1A/min to 534A/8.89V, local @ 525A/8.90V. Pressure is coming down to low 10e-6. (See attachment 3: TGHT_525A.jpg)
Increased ramping rate to 2A/min until TGHT reaches to 1000A.
Thursday, March 22, 2012, 13:32
A decision was made to stop the TGHT autoramping program, and set the current to 700A, (local at 690A). The temperature was measured to be around 1780C on the target boat, and
1500C on the Ta-heat shield. The current remained at that current for about 2 hours before it's ramping down at zero at -10A/min.
|
Thursday, March 22, 2012, 17:56, Nikita Bernier, BeO, Target boat #1, , Done, Sintering BeO pellets
|
Nikita Bernier wrote: |
Monday, March 19, 2012, 17:04
Target boat contains 4 BeO pellets with 30% PVB:
Sample, Thickness (mm), Mass (g), Density (g/cm3)
1 4.943, 0.9628, 1.265
2 4.930, 0.9685, 1.276
3 4.758, 0.9607, 1.312
4 4.979, 0.9872, 1.288
Target chamber is currently being pumped down. Leak check will be done tomorrow by turning on the cooling water for the heat shield.
Wednesday, March 21, 2012, 18:30
The Evaporator #2 backing pump (IEVAP2BP1) muffler has been connected to the exhaust system.
The auto-ramp program has been tested today and works well.
Evaporator #2 is now auto-ramping overnight at 1 A/min, up to 500 A, between 5.00e-05 and 6.00e-05 Torr.
ISAC ops have been informed of the process and they will include it in their walkaround.
|
After sintering at up to 500 A (~1000°C), the 4 BeO pellets have shrunk and feel robust. We can manipulate them with tweesers or hands. Also we can drop them from a couple of inches high and they don't break.
One of the pellets rolled to the extremity of the target boat tube and still has black traces from bad sintering on one side.
Sample, Thickness (mm), Mass (g), Diameter (mm), Density (g/cm3)
1 3.688, 0.7118, 11.231, 1.948
2 3.822, 0.7196, 11.241, 1.897
3 3.810, 0.7037, 11.188, 1.879
4 3.803, 0.7077, 11.269, 1.866
The average thickness before sintering was 4.90 mm. After sintering, 3.78 mm. Thus the average thickness loss is 1.12 mm (22.9%)
The average mass before sintering was 0.9698 g. After sintering, 0.7107 g. Thus the average mass loss is 0.2591 g (26.7%)
The average diameter before sintering was 14.35 mm. After sintering, 11.23 mm. Thus the average diameter loss is 3.12 mm (21.7%)
The average density after sintering is 1.897 g/cm3, compared to the density of BeO (3.01 g/cm3). Thus the pellets have a BeO density of 63.0%.
Evaporator #2 is now off. |
Tuesday, March 20, 2012, 14:35, John Wong, , , , Done, Evap#2 Backing up muffler not connected to the exhaust system.
|
Tuesday, March 20, 2012, 14:22
The Evaporator #2 backing pump (IEVAP2:BP1) muffler has not connected to the exhaust duct.
See attachment#1 as to where the muffler should be connected to the exhaust ducting system.
The Evaporator chamber is currently under vacuum; the BeO sintering process will be pending for now until the backing pump is properly installed.
(ISAC E-fault 5880)
Wednesday, March 21, 2012, 13:55
Edi Dalla Valle is connecting the evaporator backing scroll pump exhaust to the existing nuclear exhaust. (See attachment#2: scroll_pump_exhause.jpg). A filter is also added between the exhaust line
to prevent any back flow of oil from the Evaporator #1 backing pump (An oil pump).
Work is covered under ISAC WP# 2012-03-21-3.
The evaporator is now operational.
|
Thursday, March 01, 2012, 14:42, John Wong, , , , , IEVAP2:TGHT/TBHT max current setpoint issue
|
Thursday, March 01, 2012, 14:35
Both the IEVAP2:TBHT and IEVAP2:TGHT maximum current setpoints on the vacuum page (see page: /edl/ievap2_vacuum1.edl) are wrong.
For IEVAP2:TGHT, the maximum current setpoint should be 1500A (see page: /edl/ievap2tghtcp.edl), not 1000A.
For IEVAP2:TBHT, the maximum current setpoint should be 500A (see page: /edl/ievap2tbhtcp.edl), not 300A.
See attachement#1 for grabscreen.
Fault: 5853
|
Tuesday, February 28, 2012, 11:00, John Wong, Empty, Test oven , LP-SIS, Done, Measuring temperatures, currents & voltages
|
Tuesday, February 28, 2012, 10:36
Two thermocouples were inserted through the left side of the copper heat shield, see attachment #1. One thermocouple is attached to the target tube with a Ta-wire, and the other is attached to the back block.
Data gathering:
1. Target heater (IEVAP2:TGHT) setpoint current/voltage
2. Target heater (IEVAP2:TGHT) readback current/voltage
4. Tube heater (IEVAP2:TBHT) setpoint current/voltage
3. Thermocouples voltages & controls' readback (IEVAP2:TCM)
|
Monday, February 13, 2012, 16:24, John Wong, , , , Done, Evaporator #2 Commissioned
|
Monday, February 13, 2012, 16:21
The Evaporator 2 is now commissioned. See attachment#1 for the commissioning report or refer to Document #43321. |
Thursday, July 21, 2011, 17:33, Pierre Bricault, , , , Maintenance,
|
Rick mentioned to me that the evaporator is ready for the next steps of the commissioning process.
In the chamber only the target leg heaters have current by-pass clamps on them.
The ionizer tube heaters do not have them because these lines do not have the same configuration as the others. The current by-pass clamps will
not fit these lines.
We may not need this for the commissioning, Rick will design and manufacture something for this when I get back from holiday.
The water is on in all circuits except for the power supply cooling circuit.
Pierre |
Monday, March 28, 2011, 12:40, John Wong, , , , , Under Construction
|
Evaporator #2 is still under construction. For further information please contact Jens Lassen. |
|