Friday, June 11, 2021, 08:05
Target boat with a layer of niobium foil on the bottom is used to heat up Nb samples to 1100 C for 4 hrs.
OMEGA slope = 0.99
The niobium samples are wrapped in a layer of Nb foil.
Boat is wrapped with 2 layers of Nb foil.
Good vacuum 3.00e-02 Torr
Bad vacuum 5.00e-02 Torr
Autoramping TGHT at 2A/min to 50A then to 100A, then monitor until desired temperature
Initial IGP1= 9.4e-07 Torr
Friday, June 11, 2021, 09:59
TGHT = 200 A, 2.7V
IGP1= 9.8e-07 Torr
Tap to 1100C
Friday, June 11, 2021, 10:09
Temperature reached at 10:05 am.
TGHT = 224A, 3.1V
IGP1= 1.0e-06 Torr
OMEGA= 1100C +/- 10C fluctuations
Friday, June 11, 2021, 14:10
TGHT = 224A, 3.1V
IGP1= 9.2e-.07 Torr
OMEGA = 1100C +/- 10C fluctuations
Started rampdown at -3A/min
|