Thursday, June 11, 2020, 09:56
Previous day (Wednesday June 10, 2020)
Container coated with TaC and wrapped with 3 Ta heat shields.
Desired temperature= 1900 C, Omega Slope set = 0.990, Auto TGHT at 0.2A/min to reach 400A, TGHT will be tapped up accordingly to reach desired Temp.
TBHT will be set fixed at 230 A (max).
Good vac at 3.00e -5 Torr
Bad vac at 5.00e-5 Torr
Chamber pump down
Thursday, June 11, 2020, 10:19
IEVAP2:IGP1=1.06e-6 Torr
ramping to 40A (TGHT and TBHT) at 1A/min
Thursday, June 11, 2020, 12:35
IEVAP2:IGP1=1.8e-6 Torr
TGHT = 39.8 A, 0.45V
TBHT=38.5 A, 0.48V
Manually rampted to 45A on both TGHT and TBHT
Thursday, June 11, 2020, 12:58
IEVAP2:IGP1=1.6e-6 Torr
TGHT = 34.8 A, 0.52V
TBHT=44.2A, 0.55V
Start Autoramp at .5A/min to 400A on TGHT and 230A on TBHT
Thursday, June 11, 2020, 17:14
Irregular pressure profile. Cooling . Need to check for leak.
TGHT = 99 A 1.3 V
TBHT = 99 A 1.4 V
Friday, June 12, 2020, 12:59
Restarting ramping
IGP1= 4.98e7 Torr
Autoramp at 1A/min to 400A on TGHT and 230A on TBHT
(pressure and TGHT current and voltage profile seem normal compared to previous coating sintering with the same power supply)
Friday, June 12, 2020, 14:40
Paused ramping
TGHT = 90A
After a few minutes the profile (noise) was still there. Continue autoramp at 0.5A/min to 400 A on TGHT and 230A on TBHT
Friday, June 12, 2020, 15:21
IGP1= 1.97e-06 Torr trending down
TGHT = 111.5 A , 1.5 V
TBHT = 112.9 A, 1.9 V
Increase ramping speed to 1A/min to 400A on TGHT and 230A on TBHT
Friday, June 12, 2020, 20:50
OMEGA = 1754 C
IGP1= 2.5e-6 Torr
TGHT = 394.1 A, 6.6 V
TBHT = 232.8 A, 4.0 V
Tapping to 1900 C
Friday, June 12, 2020, 21:00
OMEGA =1901 C
IGP1= 5.6e-6 Torr
TGHT = 448.3 A, 7.5 V
TBHT = 232.8 A, 4.1 V
Saturday, June 13, 2020, 00:51
OMEGA = 1898 C
IGP1 = 2.0e-6 Torr
TGHT = 447.2 A, 7.5 V
TBHT = 232.9 A, 4.1 V
Start cooling at -2A/ min for TGHT and -1A/min for TBHT
|