John Wong wrote: |
Laura Lambert wrote: |
Thursday, June 04, 2015, 9:07
Container was sprayed with TaC and let dry.
Container has 3x Ta heat shields including center block.
Container was loaded into EVAP2 yesterday and pumped down overnight.
HS water valves were opened up this morning, no leaks detected.
IGP1 = 4.6e-7 Torr.
Tapped up manually to 40A.
Waited ~25min, Vacuum stable.
IGP1 = 5.0e-7 Torr.
Initiating auto-ramp.
TGHT will be ramped to reach 2000C
Friday, June 05, 2015, 10:01
IGP1 = 4.5e-7 Torr.
TGHT = 313A, 4.47V
OMEGA = 1444C
Increasing ramping rate to 1.0A/min
Friday, June 05, 2015, 11:31
IGP1 = 1.2e-6 Torr.
Increasing ramping rate to 2.0A/min
|
Friday, June 05, 2015, 12:01
TGHT reached to 465A/7.56V, temp is stable at 2000C. Current vac at 1.2e-6 Torr and coming down
Cooling down process can be initiated after 4 hours.
|
Friday, June 05, 2015, 13:21
OMEGA = 1995C
Increasing TGHT to 470A to achieve desired max temperature of 2000C
Friday, June 05, 2015, 15:59
TGHT sat at max desired temperature of 2000C for ~4hrs.
TGHT = 470A, 7.7V
Initiating auto-cool at 1.0A/min.
Monday, June 08, 2015, 11:31
Vented in air and opened up this morning.
Target container mostly sintered, two tiny patches near both ends not fully sintered.
Will re-install and re-sinter next week as another container with priority needs to be sintered first.
Tuesday, June 09, 2015, 10:45
See attachements for 'not-fully-sintered' photos
|