Tuesday, May 14, 2013, 17:15, John Wong, Empty, 38481-6, HP-FEBIAD, Done, SinteringTaC coating
|
Tuesday, May 14, 2013, 17:04
Target oven is coated with TaC, and wrapped with 3-Ta heat shields.
TGHT and TBHT will be ramped up to 820A and 300A, respectively. |
Tuesday, May 07, 2013, 16:53, Nikita Bernier, BeO, , , Done, Sintering BeO pellets #6
|
Tuesday, May 07, 2013, 16:48
5 BeO pellets were made. Each weights about 1.3 g (including org mass). |
Monday, May 13, 2013, 12:53, Nikita Bernier, BeO, , , Done, Sintering BeO pellets #6
|
Nikita Bernier wrote:
Tuesday, May 07, 2013, 16:48 |
Monday, May 13, 2013, 17:17, Nikita Bernier, BeO, , , Done, Sintering BeO pellets #6
|
Nikita Bernier wrote:
|
Tuesday, April 30, 2013, 11:20, Anders Mjos, Empty, 38481-5, HP-FEBIAD, Done, CTL thermal test
|
CTL block on T/C F/T Ch 1
Supply on Ch 3
HS Return on Ch 4 |
Friday, April 19, 2013, 15:27, Anders Mjos, Empty, 38481-4, HP-FEBIAD, Done, CTL test
|
Target installed with 4 T/C
The target assembly is ITD0300 with the CTL Cu cooling block slightly modified.
Ch1 - CTL cooling block T/C feedtrough |
Monday, April 22, 2013, 18:49, John Wong, Empty, 38481-4, HP-FEBIAD, Done, CTL test
|
Anders Mjos wrote:
Target installed with 4 T/C |
Tuesday, April 23, 2013, 10:11, Anders Mjos, Empty, 38481-4, HP-FEBIAD, Done, CTL test
|
John Wong wrote:
|
Friday, April 19, 2013, 09:39, Rick Maharaj, Empty, , , Done, thermocouple Feedthru
|
A thermocouple feedthru was installed via 9 pin sub-D connector. It runs from the the conflat cross on the top of the evaporator to the upper 9
pin connector of the target mounting plate. |
Thursday, April 11, 2013, 14:20, John Wong, Empty, 39165-6, LP-SIS, Done, Coating target oven /w TaC & sintering for UCx#6
|
Monday, April 08, 2013, 17:39
Target container is coated with TaC; the container will be used for the UCx#6 target.
No Ta-heat shields are used. |
Thursday, March 14, 2013, 12:27, Anders Mjos, Empty, 38481-4, HP-FEBIAD, Done, CTL thermal test 3 (w/o CTL block)
|
Thursday, March 12, 2013
The CTL was removed and target heated to 580A / 300A
T1: Left target leg close to tube |
Wednesday, March 13, 2013, 16:08, Anders Mjos, Empty, 38481-4, HP-FEBIAD, Done, Thermal test
|
Wednesday, March 13, 2013
Thermocouple channels (see attached PDF for photos)
T1 - Left target leg at tube |
Wednesday, March 06, 2013, 10:41, Anders Mjos, Empty, 38481-4, HP-FEBIAD, Done, CTL thermal test
|
Wednesday, March 06, 2013
The Cool Transfer Line (CTL) test target is installed for thermal tests. Drawing number is ITD0431 REV A.
Thermocouple channels are as follows: |
Wednesday, March 06, 2013, 17:53, John Wong, Empty, 38481-4, HP-FEBIAD, Done, CTL thermal test
|
Anders Mjos wrote:
Wednesday, March 06, 2013 |
Monday, March 11, 2013, 12:23, Anders Mjos, Empty, 38481-4, HP-FEBIAD, Done, CTL thermal test 2
|
Anders Mjos wrote:
|
Monday, March 11, 2013, 15:59, John Wong, Empty, 38481-4, HP-FEBIAD, Done, CTL thermal test 2
|
Anders Mjos wrote:
|
Monday, March 04, 2013, 17:41, John Wong, Empty, LP-SIS RFQ ver 2.0, , , Testing LPSIS RFQ ver 2.0
|
Monday, March 04, 2013, 17:39
This is the 2nd modified target container for RFQ LPSIS. The container will be heated up to 650A TGHT and 150A on TBHT. No Ta-heat
shield is being used. |
Friday, February 22, 2013, 15:55, John Wong, SiC, , LP-SIS, Done, Sintering SiC#28-RFQ
|
Friday, February 22, 2013, 15:49
The LP-SIS RFQ target container was previously coated with TaC and sintered up to ~1500C (TGHT @ 600A, TBHT @ 300A).
The container is loaded with 325 discs of SiC, a total of 10.9cm in length. |
Monday, February 18, 2013, 16:43, John Wong, Empty, , LP-SIS, Done, Sintering TaC coating on the RFQ target container
|
Monday, February 18, 2013, 16:28
The RFQ target container is coated with TaC and ready to be sintered. No Ta-heat shields are used. This container will be used for
the SiC#28-LPSIS-RFQ. |
Tuesday, January 22, 2013, 16:14, John Wong, , , LP-SIS, Done, Heating RFQ components & measuring temperatures
|
Tuesday, January 22, 2013, 12:38
This is to test the newly developed RFQ target to be commissioned this year. The purpose of this test is to see how well the RFQ components
can sustain the high temperature. One thermocouple is connected inside the target and the other is connect outside of the Cu heat-shield. RGA |
Friday, January 11, 2013, 11:16, John Wong, , , , Maintenance, Replace terminal insulator
|
Friday, January 11, 2013, 10:59
The insulator that holds the terminals was broken when a target container was installed. The insulator had seen so much heat shine from the
Cu heat-shield gaps, see attachment. Tightening the bolts on the target container might further put more force on the insulator and eventually broke |
Friday, January 11, 2013, 15:16, Anders Mjos, , , , Maintenance, Replace terminal insulator
|
John Wong wrote:
Friday, January 11, 2013, 10:59 |
Friday, January 11, 2013, 14:00, John Wong, Empty, Ta-Target boat, , Done, Testing QMS & thermocouples
|
Friday, January 11, 2013, 13:52
TEST#1
A new target boat is coated with TaC and will go through the sintering process at 580A (max). Ramping rate 5A/20min. |
Tuesday, October 16, 2012, 14:18, John Wong, TiC, 39165-4, LP-SIS, Done, Sintering TiC#3
|
Tuesday, October 16, 2012, 14:12
Target is filled with 360 discs of TiC (with 1 mole of graphite) backed on C-grv foil.
No Ta heat-shields wrapped around the container. |
Wednesday, October 10, 2012, 16:37, John Wong, Empty, 39165-4, LP-SIS, Done, Coating target oven /w TaC & sintering for TiC#3
|
Wednesday, October 10, 2012, 16:35
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min. |
Wednesday, September 26, 2012, 15:14, Nikita Bernier, BeO, , , Done, Sintering BeO Pellets #4
|
Wednesday, September 26, 2012, 15:07
The samples were made of BeO powder with 30% PVB which was treated at 400 RPM for 26 minutes. |
Friday, September 28, 2012, 12:59, Nikita Bernier, BeO, , , Done, Sintering BeO Pellets #4
|
Nikita Bernier wrote:
Wednesday, September 26, 2012, 15:07 |
Monday, September 24, 2012, 15:12, Nikita Bernier, TaC, , , Done, Sintering Ta foil with TaC coating
|
Monday, September 24, 2012, 15:01
The target boat with TaC coating is being used again. The inside of the boat is covered with a 0.002 inches thick Ta foil with TaC coating, wrapped
with a 0.002 inches thick Ta foil. |
Monday, September 24, 2012, 18:09, Nikita Bernier, TaC, , , Done, Sintering Ta foil with TaC coating
|
Nikita Bernier wrote:
Monday, September 24, 2012, 15:01 |
Wednesday, September 26, 2012, 15:06, Nikita Bernier, TaC, , , Done, Sintering Ta foil with TaC coating
|
Nikita Bernier wrote:
|
Wednesday, August 22, 2012, 17:36, John Wong, Empty, 39165-5, LP-SIS, Done, Coating target oven /w TaC & sintering for UCx#5
|
Wednesday, August 22, 2012, 17:25
Note: LP-FEBIAD target container ( W.O#37918-3) was coated with TaC and sintered on July 19 for UCx#5 target. Then, a last minute request
from the Sci Dev. to run the UCx#5 in LP-SIS. |
|