Wednesday, January 16, 2019, 11:53, Marla Cervantes, TaC, 43630-2, , Done, TaC coating/sintering for graphite insert test
|
Tuesday, January 15, 2018, 17:30
Tantalum tube was coated with TaC and wrapped with Ta heat-shield (3 layers)
Desired temp = 1900 C (expected TGHT ~445A/7.5V), TBHT will be set fixed at 230A (max). |
Wednesday, January 23, 2019, 13:06, Marla Cervantes, , 43630-2, , Done, Graphite insert test #3
|
Wednesday, January 23, 2019, 13:01
A previously coated tantalum tube with 3 layers of shielding (Details in e-log
426) was loaded with a graphite insert. |
Wednesday, February 13, 2019, 10:08, Darwin Ortiz Rosales, , 43630-1 , , Done, Graphite insert test 3b
|
Wednesday, February 13, 2019, 10:04
A previously coated tantalum tube with 3 layers of shielding (Details in e-log 426) was loaded with a graphite insert. |
Friday, May 29, 2020, 10:26, Marla Cervantes, Empty, 43044-8, LP-SIS, Done, TaC coating/sintering
|
Friday, May 29, 2020, 08:52
Ta tube was coated with TaC and wrapped with Ta heat-shields (3 layers)
Desired temperature= 1900 C (expected TGHT ~430 A), TBHT will be set fixed at 230A (max). |
Thursday, October 25, 2018, 15:37, Marla Cervantes, TaC, 43044-7, LP-SIS, Done, TaC coating/sintering for graphite insert test
|
Thursday, October 25, 2018, 10:36
Container is coated with TaC and wrapped with Ta heat-shield (3 layers)
Desired temp = 1900 C (expected TGHT ~445A/7.5V), TBHT will be set fixed at 230A (max). |
Tuesday, April 30, 2019, 09:35, Darwin Ortiz Rosales, Empty, 43044-6, LP-SIS, Done, TaC coating/sintering 
|
Tuesday, April 30, 2019, 09:33
Container was coated with TaC and wrapped with 2 Ta heat shields.
Desired temp = 1900 C, Omega slope set = 0.990, Auto ramping TGHT at 1A/min to reach 400A, |
Tuesday, July 30, 2019, 15:42, Darwin Ortiz Rosales, ZrC, 43044-6, LP-SIS, Done, Sintering ZrC Discs
|
Tuesday, July 30, 2019, 15:33
ZrC backup Target 12.6 cm disc length, 465 g total weight (no springs and no analysis discs).
Total weight= 470 g. |
Monday, August 12, 2019, 15:55, John Wong, ZrC, 43044-6, LP-SIS, Done, Sintering ZrC Discs
|
Darwin Ortiz Rosales wrote:
|
Friday, January 18, 2019, 15:11, Darwin Ortiz Rosales, Empty, 43044-5, LP-SIS, Done, TaC coating/sintering (training/online use)
|
Friday, January 18, 2019, 15:00
Container was coated with TaC and wrapped with 3 Ta heat shields.
Desired temp = 1900 C, Omega slope set = 0.990, Auto ramping TGHT at 1A/min to reach 400A, TGHT |
Monday, March 18, 2019, 15:58, Darwin Ortiz Rosales, ZrC, 43044-5, LP-SIS, Done, Sintering ZrC 
|
Monday, March 18, 2019, 15:51
Total number of foils: 555
Total mass of material including graphite foils: 478 grams |
Tuesday, April 23, 2019, 13:55, Aaron Schmidt, Ta, 43044-4, LP-SIS, In progress, Conditioning Ta#58 
|
Ta#58 LP-SIS target description:
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.025mm |
Wednesday, July 25, 2018, 17:33, John Wong, Empty, 43044-2, LP-SIS, Done, TaC coating/sintering for UCx#24
|
Wednesday, July 25, 2018, 17:32
Container is coated with TaC and wrapped with 3 layers of Ta heat-shields.
Desired sintering temperature ~1900 C, TGHT is estimated to be ~ 445A (3.3 kW), TBHT set to 230A (as usual). |
Monday, August 20, 2018, 18:10, John Wong, np-SiC, 43044-1, LP-SIS, Done, nano-SiC final conditioning
|
Monday, August 20, 2018, 17:58
14.9 g of np-SiC fibrous target discs are loaded into the container (previously coated with TaC and sintered, see elog ID 414).
Total loaded length 9.5 cm. |
Thursday, February 21, 2019, 09:15, Darwin Ortiz Rosales, Empty, 42464-4, HP-FEBIAD, Done, 
|
Thursday, February 21, 2019, 09:01
Container coated with TaC and wrapped with 2 Ta heat shields.
Desired temperature= 1900 C, Omega Slope set = 0.990, Auto TGHT at 0.2A/min to reach 400A, TGHT will be tapped up accordingly to reach desired |
Monday, June 24, 2019, 08:42, Darwin Ortiz Rosales, SiC, 42464-4, HP-FEBIAD, Done, Conditioning of BSiC discs
|
Monday, June 24, 2019, 08:24
Total number of foils: 484
Total mass in including container = 1495 grams |
Saturday, November 23, 2019, 14:03, Darwin Ortiz Rosales, TaC, 42464-3, HP-FEBIAD, Done, TaC coating/sintering
|
12.3
Saturday, November 23, 2019, 14:00
Container coated with TaC and wrapped with 3 Ta heat shields. |
Tuesday, November 26, 2019, 15:21, Darwin Ortiz Rosales, SiC, 42464-3, HP-FEBIAD, Done, Conditioning of SiC discs (sintering) (RUSH)
|
Tuesday, November 26, 2019, 14:53
Total number of foils: 504
Total length packed 17.4 cm |
Tuesday, November 26, 2019, 15:43, Anders Mjos, SiC, 42464-3, HP-FEBIAD, Problems resolved, Water to vacuum leak on heat shield line
|
This morning, the vacuum responded to shutting of the water of the heat shield circuit (leak rate without pumping leveling out). The vacuum chamber was
vented and the heat shield with flexible lines was replaced with another heat shield with fixed lines. The chamber was again pumped down and water opened
at ~150 mTorr to test the leak up rate without pumping. No leaks apparent, so continued pumping down with turbo pump. At a vacuum of about 1E-6 Torr the |
Wednesday, November 27, 2019, 17:45, John Wong, SiC, 42464-3, HP-FEBIAD, Done, Conditioning of SiC discs (sintering) (RUSH)
|
Darwin Ortiz Rosales wrote:
Tuesday, November 26, 2019, 14:53 |
Wednesday, March 09, 2022, 06:27, Darwin Ortiz Rosales, TaC, 42464-2, HP-FEBIAD, Done, TaC coating/sintering
|
Wednesday, March 09, 2022, 06:25
Ta HP-FEBIAD was coated with TaC and wrapped with Ta heat-shields (3 layers)
Desired temperature = 1800 C , TBHT will be set fixed at 230A (max). |
|