    Reply  Wednesday, August 14, 2024, 16:24, Marla Cervantes, C, 44139-5 SK, LP TUBE, In progress, EVAP2 Calibration - Vanadium  
 
 


    
        

           Marla Cervantes wrote:
        
        

           
            
            
Entry  Monday, November 07, 2022, 14:26, Darwin Ortiz Rosales, TaC, 44139-4, TARGET BOAT, Done, TaC coating sintering 
Monday, November 07, 2022, 14:24
The coated container tube was wrapped in four Ta foil heatshields.
Target temperature on OMEGA= 1850-1900 C
Entry  Wednesday, May 24, 2023, 15:23, Darwin Ortiz Rosales, , 44139-4, LP TUBE, Done, Graphite inside insert Experiment 1 Screenshot_Graphite_insert_Exp1.png
 
Wednesday, May 24, 2023, 15:22
A Ta container tube was wrapped with 4 Ta heatshields.  Note final container is 45220-11
Entry  Tuesday, June 06, 2023, 09:14, Darwin Ortiz Rosales, C, 44139-4, TARGET BOAT, Done, Graphite inside insert Experiment 2 (regular formulation discs) 
Tuesday, June 06, 2023, 09:11
A Ta container tube was wrapped with 4 Ta heatshields.  Note final container is 45220-6
272 graphite discs were loaded.
Entry  Thursday, September 29, 2022, 10:02, Darwin Ortiz Rosales, , 44139-3, TARGET BOAT, Done, 220926-Graphite conditioning in target tube 
Thursday, September 29, 2022, 09:57
A Ta container tube was wrapped with 3 Ta heatshields.
338 graphite discs were loaded.
Entry  Tuesday, October 25, 2022, 12:25, Darwin Ortiz Rosales, TaC, 44139-15-SK, LP-SIS, Done, TaC coating sintering 
Tuesday, October 25, 2022, 12:18
Container wrapped in 4 Ta foil heatshields
Target temperature on OMEGA= 1850-1900 C
Entry  Monday, June 01, 2020, 12:03, Aaron Schmidt, Ta, 44139-13, LP-SIS, In progress, Ta#60 Conditioning 
 Ta#60 LP-SIS target description:
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.025mm
Entry  Thursday, June 11, 2020, 13:01, Darwin Ortiz Rosales, Empty, 44139-12, LP-SIS, Done,  WO#_44139-12_TaC_sintering.PNG
 Thursday, June 11, 2020, 09:56
Previous day (Wednesday June 10, 2020) 
Container coated with TaC and wrapped with 3 Ta heat shields.
Entry  Wednesday, March 18, 2020, 07:21, Marla Cervantes, TaC, 44139-11, LP-SIS, Done, TaC coating/sintering IMG_1538.JPG
 Wednesday, March 18, 2020, 07:10
Ta tube was coated with TaC and wrapped with Ta heat-shields (3 layers)
Desired temperature= 1900 C (expected TGHT ~430 A), TBHT will be set fixed at 230A (max).
Entry  Sunday, May 24, 2020, 13:39, Marla Cervantes, Empty, 44139-11, LP-SIS, Done, TaC coating/sintering  TaC-coating-sintering.PNG
 Sunday, May 24, 2020, 06:54
Ta tube was coated with TaC and wrapped with Ta heat-shields (3 layers)
Desired temperature= 1900 C (expected TGHT ~430 A), TBHT will be set fixed at 230A (max).
Entry  Thursday, July 16, 2020, 11:15, Darwin Ortiz Rosales, SiC, 44139-11, LP-SIS, Done, SiC sintering for Luca 1 of 2 
 Thursday, July 16, 2020, 11:15
Coated Ta tube cotaining 233 SiC disks wrapped with Ta heat-shields (3 layers)
Desired temperature= 1800C (expected TGHT 410 A), TBHT will be set fixed at 230A (max).
Entry  Monday, July 20, 2020, 19:25, Darwin Ortiz Rosales, SiC, 44139-11, LP-SIS, Done, SiC sintering for Luca 2 of 2 
Monday, July 20, 2020, 19:27 
Coated Ta tube cotaining 355 SiC disks wrapped with Ta heat-shields (3 layers)
Desired temperature= 1800C (expected TGHT 410 A), TBHT will be set fixed at 230A (max).
Entry  Thursday, April 08, 2021, 08:25, Aaron Schmidt, Ta, 44139-10, LP-SIS, In progress, Conditioning Ta#62 & Flex - line HS installed 
 Ta#62 LP-SIS target description:
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.025mm
Entry  Thursday, October 03, 2019, 09:26, Darwin Ortiz Rosales, TaC, 44062-6, LP-SIS, Done, TaC coating/sintering 
Thursday, October 03, 2019, 08:58
Ta tube was coated with TaC and wrapped with Ta heat-shields (3 layers)
Initial weight including heat-shields = 427 g
Entry  Monday, September 16, 2019, 14:50, Aaron Schmidt, Ta, 44062-5, LP-SIS, In progress, Conditioning Ta#59 Ta#59_Evap_2_Conditioning..docx
 Ta#59 LP-SIS target description:
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.025mm
Entry  Friday, September 06, 2019, 11:58, Darwin Ortiz Rosales, , 44062-4, LP-SIS, Done, TaC coating/sintering 190906LPSIS_Sintering.PNG
Friday, September 06, 2019, 11:20
Container was coated with Tac and wrapped with 2 Ta heat shields.
Desired temp=1900 C, Omega slope set =0.990
Entry  Wednesday, September 11, 2019, 15:16, Marla Cervantes, , 44062-4, LP-SIS, Done, TaC coated target container calibration/conditioning  A.JPGB.JPG
 Wednesday, September 11, 2019, 15:12
A target container coated with TaC elog 455 was loaded with an empty graphite
cartridge and set it in the EVAP2
Entry  Thursday, October 17, 2019, 13:53, Darwin Ortiz Rosales, TaC, 44062-3, LP-SIS, In progress, TaC coating/sintering 
Thursday, October 17, 2019, 12:00
Ta tube was coated with TaC and wrapped with Ta heat-shields (3 layers)
Desired temperature= 1900 C (expected TGHT ~430 A), TBHT will be set fixed at 230A (max).
Entry  Wednesday, August 28, 2019, 05:59, Marla Cervantes, , 44062-2-SK, , Done, Graphite insert test 
Wednesday, August 28, 2019, 06:00
A graphite insert (with conical caps) was loaded in tantalum tube 
the Ta tube was wrapped with 3 tantalum foils,
Entry  Friday, May 24, 2019, 15:29, Marla Cervantes, , 43943-2, , Done, Graphite insert test 
Friday, May 24, 2019, 15:26
 A graphite insert with tantalum wires in its caps
was loaded in a tantalum tube, the system will be heated to 2000 C