Logbooks Lab Maintenance Evaporator_1 Evaporator_2 Laser cutter Target Production Test-Stand RH-ISAC RH-Cyclotron RH-Meson Hall RH-Beamlines RH-ARIEL
  Evaporator_2, Page 8 of 34  Not logged in ELOG logo
Entry  Tuesday, May 19, 2015, 13:54, Laura Lambert, Empty, 41177-1, LP-SIS, Done, Sintering TaC coating container for ZrC 
 Tuesday, May 19, 2015, 13:33
Target container is coated with TaC.  No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min.
Entry  Friday, May 22, 2015, 11:44, Laura Lambert, Empty, , TARGET BOAT, In progress, Sintering TaC coating on Ta target boat 
 Friday, May 22, 2015, 11:43
A target boat was sprayed with TaC coating and let dry yesterday.
The target boat is wrapped with 3-layers of Ta-heat shield.
    Reply  Tuesday, May 26, 2015, 13:05, Laura Lambert, Empty, 40282-5, TARGET BOAT, Done, Sintering TaC coating on Ta target boat target_boat_-_may_22.jpg


    
        
            John Wong wrote:
        
        
            
            
            
Entry  Tuesday, May 26, 2015, 13:57, Laura Lambert, Endcaps, 40282-5, TARGET BOAT, In progress, Sintering TaC coating on Ta endcaps endcaps_-_may_26.jpg
 Tuesday, May 26, 2015, 13:06
Endcaps were sprayed with TaC coating and let dry.
Each endcap is wrapped separately with a sheet of graphite foil and stacked in the target boat [see image]
    Reply  Thursday, May 28, 2015, 10:23, Laura Lambert, Endcaps, 40282-5, TARGET BOAT, Problems, Sintering TaC coating on Ta endcaps - not fully sintered endcaps_-_round1_sintering_(1).jpgendcaps_-_round1_sintering_(2).jpg


    
        
            John Wong wrote:
        
        
            
            
            
Entry  Thursday, May 28, 2015, 11:36, Laura Lambert, Endcaps, 40282-5, TARGET BOAT, In progress, Sintering TaC coating on Ta endcaps - round 2 endcaps_-_may_28_-_round2.jpg
 Thursday, May 28, 2015, 11:34
Endcaps were sintered [see elog#199]
A Ta foil is placed in the target boat with separate slots for each endcap [see image]
    Reply  Friday, May 29, 2015, 11:18, Laura Lambert, Endcaps, 40282-5, TARGET BOAT, Done, Sintering TaC coating on Ta endcaps - round 2 endcaps_-round2_sintering_(1).jpgendcaps_-round2_sintering_(2).jpg


    
        
            John Wong wrote:
        
        
            
            
            
Entry  Friday, May 29, 2015, 11:29, Laura Lambert, ZrC, 41177-1, LP-SIS, In progress, Conditioning ZrC#7 
 Friday, May 29, 2015, 11:21
Total number of foils: 425 discs
Total mass of materials [incl graphite foils]: 44.41g
    Reply  Wednesday, June 03, 2015, 10:47, Laura Lambert, ZrC, 41177-1, LP-SIS, Done, Conditioning ZrC#7 Conditioning_target_-_no_heat_shields-no_endcaps.xlsx


    
        
            John Wong wrote:
        
        
            
            
            
Entry  Thursday, June 04, 2015, 11:10, Laura Lambert, Empty, , LP-IG-LIS, In progress, Sintering TaC coating container for UCx 
 Thursday, June 04, 2015, 9:07
Container was sprayed with TaC and let dry.
Container has 3x Ta heat shields including center block.
    Reply  Friday, June 05, 2015, 13:22, Laura Lambert, Empty, 40860-1, LP-IG-LIS, In progress, Sintering TaC coating container for UCx IMG_20150608_145926159.jpgIMG_20150608_145950384.jpg


    
        
            John Wong wrote:
        
        
            
            
            
Entry  Tuesday, June 09, 2015, 10:44, Laura Lambert, Empty, 41177-2, LP-SIS, In progress, Sintering TaC coating container for ZrC back-up 
 Tuesday, June 09, 2015, 9:16
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min.
    Reply  Thursday, June 11, 2015, 16:10, Laura Lambert, Empty, 41177-2, LP-SIS, In progress, Sintering TaC coating container for ZrC back-up 


    
        
            John Wong wrote:
        
        
            
            
            
    Reply  Friday, June 12, 2015, 14:59, Laura Lambert, Empty, 40860-1, LP-IG-LIS, In progress, Sintering TaC coating container for UCx 


    
        
            John Wong wrote:
        
        
            
            
            
    Reply  Tuesday, June 23, 2015, 10:18, Laura Lambert, Empty, 38817-6, HP-SIS, Done, RUSH! Sintering TaC coated container for SiC  


    
        
            John Wong wrote:
        
        
            
            Monday, June 22, 2015, 13:00
    Reply  Thursday, June 25, 2015, 16:13, Laura Lambert, SiC, 38817-6, HP-SIS, Done, RUSH! SiC backup target undergoes sintering process IMG_20150625_152233125.jpgIMG_20150625_152256456.jpg


    
        
            John Wong wrote:
        
        
            
            Tuesday, June 23, 2015, 12:21
Entry  Thursday, June 25, 2015, 16:20, Laura Lambert, ZrC, 41177-2, LP-SIS, In progress, Sintering back-up ZrC 
 Thursday, June 25, 2015, 16:14
Total number of foils: 422 discs
Total mass of materials [incl graphite foils]: 
Entry  Monday, June 29, 2015, 16:18, Laura Lambert, Empty, 41369-2, LP-SIS, In progress, Sintering TaC coating container 
 Monday, June 29, 2015, 16:17
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min.
    Reply  Tuesday, June 30, 2015, 09:50, Laura Lambert, Empty, 41369-2, LP-SIS, In progress, Sintering TaC coating container LP-SIS_july3_2015_(1).jpgLP-SIS_july3_2015_(2).jpgLP-SIS_july3_2015_(3).jpgLP-SIS_july3_2015_(4).jpg


    
        
            John Wong wrote:
        
        
            
            
            
    Reply  Monday, July 06, 2015, 16:30, Laura Lambert, Empty, 41369-2, LP-SIS, Done, Sintering TaC coating container July_10_2015_-_2nd_round_sintering_-_coating_(1).jpgJuly_10_2015_-_2nd_round_sintering_-_coating_(2).jpgJuly_10_2015_-_2nd_round_sintering_-_coating_(3).jpgJuly_10_2015_-_2nd_round_sintering_-_coating_(4).jpg


    
        
            John Wong wrote:
        
        
            
            
            