Monday, June 15, 2015, 15:30, John Wong, Empty, 41177-2, LP-SIS, Done, Re-Sintering TaC coating container for ZrC back-up
|
Laura Lambert wrote:
|
Monday, June 22, 2015, 13:11, John Wong, Empty, 38817-6, HP-SIS, In progress, RUSH! Sintering TaC coated container for SiC
|
Monday, June 22, 2015, 13:00
Containers is coated with TaC. Wrapped with 3 layers of Ta heat-shield. Air blown to for quick dry.
Installed, and pumped down, vac currently at 6.7e-6 Torr. |
Tuesday, June 23, 2015, 10:18, Laura Lambert, Empty, 38817-6, HP-SIS, Done, RUSH! Sintering TaC coated container for SiC
|
John Wong wrote:
Monday, June 22, 2015, 13:00 |
Monday, June 29, 2015, 16:18, Laura Lambert, Empty, 41369-2, LP-SIS, In progress, Sintering TaC coating container
|
Monday, June 29, 2015, 16:17
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min. |
Monday, June 29, 2015, 23:42, John Wong, Empty, 41369-2, LP-SIS, In progress, Sintering TaC coating container
|
Laura Lambert wrote:
Monday, June 29, 2015, 16:17 |
Tuesday, June 30, 2015, 09:50, Laura Lambert, Empty, 41369-2, LP-SIS, In progress, Sintering TaC coating container
|
John Wong wrote:
|
Monday, July 06, 2015, 12:07, John Wong, Empty, 41369-2, LP-SIS, In progress, Sintering TaC coating container
|
Laura Lambert wrote:
|
Monday, July 06, 2015, 16:30, Laura Lambert, Empty, 41369-2, LP-SIS, Done, Sintering TaC coating container
|
John Wong wrote:
|
Tuesday, August 25, 2015, 11:54, Laura Lambert, Empty, , HP-FEBIAD, In progress, Sintering TaC coating container for SiC Target
|
Tuesday, August 25, 2015, 11:50
Container coated with TaC using new method: Ends tapped off, with liquid poured in and swirled around entire container, then poured back
out - 'flushing technique' |
Thursday, August 27, 2015, 16:37, John Wong, Empty, , HP-FEBIAD, Done, Sintering TaC coating container for SiC Target
|
Laura Lambert wrote:
Tuesday, August 25, 2015, 11:50 |
Thursday, September 24, 2015, 09:48, Laura Lambert, Empty, 41077-5, , In progress, Sintering TaC coating container for UCx Target
|
Thursday, September 24, 2015, 08:39
IGP1 = 6.5e-7Torr
HS water valves opened, no leaks detected. |
Thursday, September 24, 2015, 12:18, John Wong, Empty, 41077-5, LP-SIS, Done, Sintering TaC coating container for UCx Target
|
Laura Lambert wrote:
Thursday, September 24, 2015, 08:39 |
Tuesday, October 06, 2015, 15:18, John Wong, Empty, 41077-5, LP-SIS, In progress, Test#1: Measuring temp with thermocouple (centre) & 2C-IR
|
John Wong wrote:
|
Thursday, October 08, 2015, 12:26, John Wong, Empty, 41077-5, LP-SIS, In progress, Test#2: Measuring temp with thermocouple (away from centre) & 2C-IR
|
John Wong wrote:
|
Wednesday, October 21, 2015, 17:39, John Wong, Empty, 41077-3, LP-SIS, In progress, Sintering TaC on LPSIS (small block) container
|
Wednesday, October 21, 2015, 17:35
This container is prepared for a backup UCx target (otherwise it will be used for development purposes).
The container is coated with TaC; one layer of Ta-heat shield is used. |
Thursday, October 22, 2015, 11:41, Laura Lambert, Empty, 41077-3, LP-SIS, In progress, Sintering TaC on LPSIS (small block) container
|
John Wong wrote:
Wednesday, October 21, 2015, 17:35 |
Thursday, October 22, 2015, 17:10, John Wong, Empty, 41077-3, LP-SIS, In progress, Sintering TaC on LPSIS (small block) container
|
Laura Lambert wrote:
|
Monday, October 26, 2015, 16:14, Laura Lambert, Empty, 41077-3, LP-SIS, Done, Sintering TaC on LPSIS (small block) container & temp measurements with 1xTa h.s
|
John Wong wrote:
|
Monday, October 26, 2015, 16:17, Laura Lambert, Empty, 41077-3, LP-SIS, Done, temp measurements with 2xTa h.s on LPSIS (small block) container 6x
|
Monday, October 26, 2015, 16:16
Container previously sintered with TaC coating and temperature measurements taken with 1x Ta heat shield [see elog ID# 256]
2x Ta heat shields on this container. |
Monday, November 02, 2015, 16:29, Laura Lambert, Empty, 41077-3, LP-SIS, Done, temp measurements with 3xTa h.s on LPSIS (small block) container
|
Monday, November 02, 2015, 16:28
Container previously sintered with TaC coating and temperature measurements taken with 1x Ta
heat shield [see elog ID# 256] and 2x Ta heat shield [see elog ID#257] |
|