Thursday, June 21, 2012, 18:13, John Wong, NiO, Ta target boat, , Failed, NiO development - Container broke!
|
John Wong wrote:
|
Sunday, April 17, 2022, 10:37, Ferran Boix Pamies, Empty, Ta boat used for annealing, TARGET BOAT, Done, PEEK samples heat test
|
Thursday, April 14, 2022, 10:36 Setup, PEEK samples installed on heatshield with TC. Pump down over the weekend.
Sunday, April 17, 2022, 10:37 Vacuum 3e-7T, ramp up TGHT 1A/10s to 500A
Sunday, April 17, 2022, 12:00 500A reached, waiting 1hour. TC at 42degC. |
Monday, April 25, 2022, 08:31, Ferran Boix Pamies, Empty, Ta boat used for annealing, TARGET BOAT, Done, PEEK sample test 2
|
Setup in vacuum over the weekend.
Monday, April 25, 2022, 08:31 IGP1:6.7e-7T . Ramping up 1A/10s to 500A.
Monday, April 25, 2022, 10:05 500A reached, waiting 1h. TC at 50degC |
Sunday, March 28, 2021, 11:24, Marla Cervantes, , NA (Ta-tube), , Done, Re-coat 3
|
Objective: Coating the inner surface of a tantalum tube to make a destructive test and use a reference for the tantalum boats coatings
Results: The tube was coated
Sunday, March 28, 2021, 11:23 |
Tuesday, April 13, 2021, 10:44, Marla Cervantes, Empty, NA (Ta- tube Eagle Alloys), , Done, Re-coat 4
|
Tuesday, April 13, 2021, 09:51
IGP1 = 2.5e-7 Torr
Tuesday, April 13, 2021, 10:17 |
Tuesday, February 23, 2021, 08:59, Marla Cervantes, , NA (Cu-tube), , Done, Re coating Test 2
|
Tuesday, February 23, 2021, 08:49
Yesterday a heat shield was washed and when dry it was installed in the EVAP2,
A 1mm thick rhenium wire was held within two copper brackets to pass through a Cu tube with the intention of coating its inside face |
Thursday, March 25, 2021, 11:24, Marla Cervantes, Empty, NA (Cu-Tube, , Done, Re-coat test 4
|
Objective: Coating the inner surface of a short tantalum tube with rhenium.
Result:
The wire snnaped around 376 W (53 A, and 7.09 V) and 2170 °C (measured with filament pyrometer)
The tube is coated
|
Tuesday, February 09, 2021, 06:48, Aaron Schmidt, , NA, , Done, Ta coating test
|
Monday, February 08, 2021, 17:00: Installed brackets w/ Ta wire and a small piece of Re to test voltage drop.
Rough down, TP on. Waterlines open.
Tuesday, February 09, 2021, 06:44: Vacuum @ 8.63e-07T. |
Thursday, February 11, 2021, 10:57, Marla Cervantes, , NA, , Done, Re coating Test 1
|
Thursday, February 10, 2021, 12:00
Objective: Heat a Re wire to evaporate it and deposit a layer of Re on the inner surface of a Ta tube.
A Re wire of 1mm diameter was clamped with Cu brackets in EVAP2, the wire is partially enclosed in a Ta tube. EVAP2 pumping down |
Monday, March 04, 2013, 17:41, John Wong, Empty, LP-SIS RFQ ver 2.0, , , Testing LPSIS RFQ ver 2.0
|
Monday, March 04, 2013, 17:39
This is the 2nd modified target container for RFQ LPSIS. The container will be heated up to 650A TGHT and 150A on TBHT. No Ta-heat
shield is being used. |
Friday, April 28, 2023, 11:31, Darwin Ortiz Rosales, TaC, Boat, TARGET BOAT, Done, TaC coated endcaps and spring sintering
|
Friday, April 28, 2023, 11:29
loaded 14 TaC coated end caps and 2 TaC coated springs.
OMEGA Slope 0.99 |
Monday, June 17, 2019, 17:09, Marla Cervantes, , 49044-9, LP-SIS, Done, Target container calibration/conditioning
|
Monday, June 17, 2019, 17:04
A LP-SIS target container was wrapped with 3 heat shielding layers,
and an empty graphite insert of 17.4 g was introduce in it. |
Thursday, August 24, 2023, 14:18, Aaron Schmidt, Nb, 45447-9, LP-IG-LIS, In progress, Conditioning Nb#11
|
Nb#11 LP-IG-LIS target description:
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.025mm (0.001") |
Friday, August 30, 2024, 11:33, Darwin Ortiz Rosales, Ta, 45447-8, LP-IG-LIS, Done, TaC coating sintering
|
Friday, August 30, 2024, 11:31
The coated container was wrapped in 4 Ta foil heatshields.
Vacuum IGP1 initial =3.1 e-07 Torr |
Wednesday, June 21, 2023, 10:37, Aaron Schmidt, Nb, 45447-7, LP-IG-LIS, In progress, Conditioning Nb#10
|
Nb#10 LP-IG-LIS target description:
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.025mm (0.001") |
Thursday, August 31, 2023, 07:09, Darwin Ortiz Rosales, TaC, 45447-4, HP-FEBIAD, Done, TaC coating sintering
|
Thursday, August 31, 2023, 07:07
The coated container was wrapped in 3 Ta foil heatshields.
Target temperature on OMEGA= 1850-1900 C |
Wednesday, December 06, 2023, 09:57, Darwin Ortiz Rosales, SiC, 45447-4, HP-FEBIAD, Done, 231204SiC conditioning
|
Wednesday, December 06, 2023, 09:47
Target number of foils:370
Analysis discs 16 A and 16B interspersed on the end further from the laser |
Friday, April 26, 2024, 06:19, Darwin Ortiz Rosales, TaC, 45447-29, HP-SIS, Done, TaC coating sintering
|
Monday, April 29, 2024, 19:50
Started coating with coating stand. |
Monday, July 22, 2024, 14:59, Aaron Schmidt, Ta, 45447-14, LP-SIS, In progress, Conditioning Ta#67 Thin foil
|
Ta#67 Thin foil LP-SIS target
description:
Total Ta foils = 470 loaded into 2 packs of 235 foils each. |
Saturday, September 07, 2024, 09:55, Darwin Ortiz Rosales, TaC, 45447-13, LP-SIS, Done, TaC coating sintering
|
Saturday, September 07, 2024, 09:54
The coated container was wrapped in 4 Ta foil heatshields.
Vacuum IGP1 initial =8.1 e-07 Torr |
|