133
|
Monday, June 09, 2014, 13:56 |
Cameron Hodgins | | | TARGET BOAT | In progress | Sintering several carbides on tantalum foil backing | Manually changed current from 500 to 615
A, monitoring the temperature. Temperature
went from 1657 C up to 1838 C. Pressure increased |
|
|
134
|
Monday, June 09, 2014, 17:15 |
Cameron Hodgins | | | TARGET BOAT | In progress | Sintering several carbides on tantalum foil backing | Target boat is now being cooled at
1 A/min from the starting point (616 A) down
to 0 A. |
|
|
150
|
Tuesday, August 05, 2014, 13:13 |
Laura Lambert | Empty | | TARGET BOAT | In progress | Sintering TaC coated end caps | Tuesday, August 05, 2014, 12:02
The target container end caps were
coated with TaC spray and let dry. |
|
|
151
|
Tuesday, August 05, 2014, 17:20 |
John Wong | | | TARGET BOAT | In progress | Sintering TaC coated end caps |
|
|
|
153
|
Thursday, August 07, 2014, 10:13 |
Laura Lambert | | | TARGET BOAT | Failed | Sintering TaC coated end caps |
|
|
|
155
|
Thursday, September 11, 2014, 14:23 |
Laura Lambert | | 40282-3 | TARGET BOAT | Failed | Sintering TaC coated end caps | Thursday, September 11, 2014, 13:14
The target container end caps were
coated with TaC spray and let dry. |
|
|
156
|
Tuesday, September 23, 2014, 15:02 |
Laura Lambert | Empty | 40282-5 | TARGET BOAT | In progress | Sintering Ta target boat with TaC coating | Tuesday, September 23, 2014, 15:00
A new target boat [new design with
no end caps] was sprayed with TaC coating |
|
|
157
|
Tuesday, September 23, 2014, 18:32 |
John Wong | Empty | 40282-5 | TARGET BOAT | Done | Sintering Ta target boat with TaC coating (with Temp measurement) |
|
|
|
158
|
Thursday, September 25, 2014, 17:35 |
John Wong | Endcaps | 40282-5 | TARGET BOAT | Done | Sintering Ta-coated endcaps (temp measured) | Thursday, September 25, 2014, 17:32
Target boat is filled with Ta-coated
endcaps. The caps are stacked together. |
|
|
164
|
Thursday, October 09, 2014, 15:59 |
John Wong | Nb | | TARGET BOAT | In progress | Conditioning Nb target (for Bob) | Thursday, October 09, 2014, 15:56
The target boat contains 5 samples
of Nb discs. Each disc is wrapped with |
|
|
166
|
Thursday, October 09, 2014, 17:41 |
John Wong | Nb | | TARGET BOAT | Done | Conditioning Nb targets (for Bob) | Thursday, October 09, 2014, 17:36
Target boat consists of 5 Nb discs.
Each disc is wrapped with Nb foil, and to |
|
|
168
|
Tuesday, November 04, 2014, 16:20 |
John Wong | SiC | | TARGET BOAT | In progress | TEST: Fabrication of SiC & Determine phase transformation 3C vs 6H | Tuesday, November 04, 2014, 16:08
The purpose of this experiment is
to improve the fabrication of SiC. |
|
|
188
|
Friday, May 01, 2015, 10:50 |
Laura Lambert | | 40282-4 | TARGET BOAT | In progress | Sintering four different ZrC samples | Friday, May 01, 2015, 10:27
Four different samples of ZrC are
loaded into a target boat. |
|
|
189
|
Monday, May 04, 2015, 17:26 |
John Wong | | 40282-4 | TARGET BOAT | In progress | Sintering four different ZrC samples |
|
|
|
190
|
Wednesday, May 06, 2015, 13:59 |
Laura Lambert | | 40282-4 | TARGET BOAT | Done | Sintering two different ZrC samples | Wednesday, May 06, 2015, 13:54
Two different samples of ZrC are
wrapped in graphite sheet and loaded into |
|
|
191
|
Friday, May 08, 2015, 15:56 |
Laura Lambert | | 40282-4 | TARGET BOAT | Done | Sintering four different ZrC samples |
|
|
|
192
|
Wednesday, May 13, 2015, 16:01 |
Laura Lambert | | 40282-4 | TARGET BOAT | Done | Sintering three different ZrC samples | Wednesday, May 13, 2015, 15:21
Three different samples of ZrC |
|
|
194
|
Friday, May 22, 2015, 11:44 |
Laura Lambert | Empty | | TARGET BOAT | In progress | Sintering TaC coating on Ta target boat | Friday, May 22, 2015, 11:43
A target boat was sprayed with |
|
|
195
|
Monday, May 25, 2015, 17:08 |
John Wong | Empty | 40282-5 | TARGET BOAT | In progress | Sintering TaC coating on Ta target boat |
|
|
|
196
|
Tuesday, May 26, 2015, 13:05 |
Laura Lambert | Empty | 40282-5 | TARGET BOAT | Done | Sintering TaC coating on Ta target boat |
|
|