Monday, June 09, 2014, 13:56, Cameron Hodgins, , , TARGET BOAT, In progress, Sintering several carbides on tantalum foil backing
|
Manually changed current from 500 to 615 A, monitoring the temperature. Temperature went from 1657 C up to 1838 C. Pressure increased up to 7.2e-7 T.
Samples should be left for about 4 hours (615 A started just before 13:00), then the goal is to ramp current back to zero. |
Monday, June 09, 2014, 17:15, Cameron Hodgins, , , TARGET BOAT, In progress, Sintering several carbides on tantalum foil backing
|
Target boat is now being cooled at 1 A/min from the starting point (616 A) down to 0 A. |
Tuesday, August 05, 2014, 13:13, Laura Lambert, Empty, , TARGET BOAT, In progress, Sintering TaC coated end caps
|
Tuesday, August 05, 2014, 12:02
The target container end caps were coated with TaC spray and let dry.
The caps are inserted in the target boat vertically, wrapped in graphite foil with 3 x Ta-heat shield. [see attached photo] |
Tuesday, August 05, 2014, 17:20, John Wong, , , TARGET BOAT, In progress, Sintering TaC coated end caps
|
Laura Lambert wrote:
Tuesday, August 05, 2014, 12:02 |
Thursday, August 07, 2014, 10:13, Laura Lambert, , , TARGET BOAT, Failed, Sintering TaC coated end caps
|
John Wong wrote:
|
Thursday, September 11, 2014, 14:23, Laura Lambert, , 40282-3, TARGET BOAT, Failed, Sintering TaC coated end caps
|
Thursday, September 11, 2014, 13:14
The target container end caps were coated with TaC spray and let dry.
The caps are inserted in the target boat wrapped in graphite foil with 3 x Ta-heat shields. |
Tuesday, September 23, 2014, 15:02, Laura Lambert, Empty, 40282-5, TARGET BOAT, In progress, Sintering Ta target boat with TaC coating
|
Tuesday, September 23, 2014, 15:00
A new target boat [new design with no end caps] was sprayed with TaC coating and let dry.
The target boat is wrapped with 3-layers of Ta-heat shield. |
Tuesday, September 23, 2014, 18:32, John Wong, Empty, 40282-5, TARGET BOAT, Done, Sintering Ta target boat with TaC coating (with Temp measurement)
|
Laura Lambert wrote:
Tuesday, September 23, 2014, 15:00 |
Thursday, September 25, 2014, 17:35, John Wong, Endcaps, 40282-5, TARGET BOAT, Done, Sintering Ta-coated endcaps (temp measured)
|
Thursday, September 25, 2014, 17:32
Target boat is filled with Ta-coated endcaps. The caps are stacked together. In between each cap, a piece of graphite foil is used
for separation so the Ta caps would not fused. |
Thursday, October 09, 2014, 15:59, John Wong, Nb, , TARGET BOAT, In progress, Conditioning Nb target (for Bob)
|
Thursday, October 09, 2014, 15:56
The target boat contains 5 samples of Nb discs. Each disc is wrapped with Nb foil and labelled.
Samples will be heated up to 1400C for 4 hours. |
Thursday, October 09, 2014, 17:41, John Wong, Nb, , TARGET BOAT, Done, Conditioning Nb targets (for Bob)
|
Thursday, October 09, 2014, 17:36
Target boat consists of 5 Nb discs. Each disc is wrapped with Nb foil, and to be heated to 1400C for 4 hours.
Chamber has been pumped down to 6.5e-7 Torr. HS valves open - no leaks detected. |
Tuesday, November 04, 2014, 16:20, John Wong, SiC, , TARGET BOAT, In progress, TEST: Fabrication of SiC & Determine phase transformation 3C vs 6H
|
Tuesday, November 04, 2014, 16:08
The purpose of this experiment is to improve the fabrication of SiC. Previously, the SiC target was heated to 2000c and yellow crystals were
observed. |
Friday, May 01, 2015, 10:50, Laura Lambert, , 40282-4, TARGET BOAT, In progress, Sintering four different ZrC samples
|
Friday, May 01, 2015, 10:27
Four different samples of ZrC are loaded into a target boat.
Sample A: ZrC + NO graphite / hand cut |
Monday, May 04, 2015, 17:26, John Wong, , 40282-4, TARGET BOAT, In progress, Sintering four different ZrC samples
|
Laura Lambert wrote:
Friday, May 01, 2015, 10:27 |
Wednesday, May 06, 2015, 13:59, Laura Lambert, , 40282-4, TARGET BOAT, Done, Sintering two different ZrC samples
|
Wednesday, May 06, 2015, 13:54
Two different samples of ZrC are wrapped in graphite sheet and loaded into the target boat.
Sample #1 = ZrC |
Friday, May 08, 2015, 15:56, Laura Lambert, , 40282-4, TARGET BOAT, Done, Sintering four different ZrC samples
|
John Wong wrote:
|
Wednesday, May 13, 2015, 16:01, Laura Lambert, , 40282-4, TARGET BOAT, Done, Sintering three different ZrC samples
|
Wednesday, May 13, 2015, 15:21
Three different samples of ZrC are loaded into a target boat.
Sample A: ZrC + NO graphite |
Friday, May 22, 2015, 11:44, Laura Lambert, Empty, , TARGET BOAT, In progress, Sintering TaC coating on Ta target boat
|
Friday, May 22, 2015, 11:43
A target boat was sprayed with TaC coating and let dry yesterday.
The target boat is wrapped with 3-layers of Ta-heat shield. |
Monday, May 25, 2015, 17:08, John Wong, Empty, 40282-5, TARGET BOAT, In progress, Sintering TaC coating on Ta target boat
|
Laura Lambert wrote:
Friday, May 22, 2015, 11:43 |
Tuesday, May 26, 2015, 13:05, Laura Lambert, Empty, 40282-5, TARGET BOAT, Done, Sintering TaC coating on Ta target boat
|
John Wong wrote:
|
|