Tuesday, April 26, 2016, 13:50, Laura Lambert, Empty, 40860-2, LP-IG-LIS, Done, sintering TaC coating on UCx#16 container
|
Tuesday, April 26, 2016, 13:32
Container coated with TaC using 'flushing technique'.
Wrapped with 3 x Ta heat shields, incl center block - new method of each layer being one long |
Tuesday, May 10, 2016, 11:57, Laura Lambert, , 40282-3, TARGET BOAT, Done, Conditioning Nb samples for Tobias
|
John Wong wrote:
|
Wednesday, May 11, 2016, 17:24, John Wong, np-SiC, , TARGET BOAT, Done, Temperature Treament of Nanofiber SiC/PAN
|
Wednesday, May 11, 2016, 17:15
Nanofiber SiC (~50nm grain size)/PAN was prepared at UBC.
SiC 0.50g, DMF 9.0g, PAN 1.0g, tiny bit of SDS. |
Tuesday, May 31, 2016, 11:10, John Wong, Empty, 41369-4, HP-SIS, Done, sintering TaC coating on SiC#33 container
|
Laura Lambert wrote:
Wednesday, May 25, 2016, 11:37 |
Thursday, June 16, 2016, 10:58, Laura Lambert, SiC, 41369-4, HP-SIS, Done, Sintering SiC#33 - 1st beta-SiC target!
|
John Wong wrote:
|
Thursday, June 16, 2016, 11:01, Laura Lambert, SiC, 41369-4, HP-SIS, Done, Conditioning SiC#33 - 1st beta SiC target! 9x
|
Thursday, June 16, 2016, 10:59
Previously sintered over weekend [see elog i.d 306]
Target container contains 450 discs of SiC [4 x 5 packs + 430 single discs] |
Monday, June 27, 2016, 11:08, Laura Lambert, Empty, 41790-3, LP-SIS, Done, sintering TaC coating on UCx#17 container
|
Monday, June 27, 2016, 11:07
Container coated with TaC using 'flushing technique'.
Wrapped with 3 x Ta heat shields, incl center block - new method of each layer being one long |
Friday, July 15, 2016, 11:52, Laura Lambert, Empty, 40860-3, LP-IG-LIS, Done, sintering TaC coating on SiC#34 container
|
Friday, July 15, 2016, 11:49
Container previously coated with TaC using 'flushing technique', cleaned ionizer tube with acetone,
so no coating inside ionizer tube |
Tuesday, July 26, 2016, 16:53, Laura Lambert, Ta, 41369-6, HP-SIS, Done, Conditioning Ta#49
|
Tuesday, July 26, 2016, 16:50
loaded into evap2
pumped down, HS water valves opened, no leaks detected. |
Tuesday, August 02, 2016, 13:56, Laura Lambert, SiC, 40860-3, LP-IG-LIS, Done, Sintering SiC#34
|
Tuesday, August 02, 2016, 13:41
Target container contains 471 discs of SiC [6 x 5 packs + 441 single discs]
Target packed length = 16cm. |
Tuesday, August 23, 2016, 12:15, John Wong, Empty, 39814-V2-1, LP-IG-LIS, Done, sintering TaC coating on SiC#34 container...round2
|
Laura Lambert wrote:
Wednesday, August 17, 2016, 17:30 |
Wednesday, August 24, 2016, 17:07, John Wong, SiC, 39814-V2-1, LP-IG-LIS, Done, Sintering process for SiC#34 (2nd round) 10x
|
Wednesday, August 24, 2016, 17:05
Target container was previously coated with TaC and sintered up to 1900C at 420A/7.01V
Container is loaded with beta-SiC 432 discs at 16cm in length. |
Monday, September 12, 2016, 17:27, John Wong, Empty, 39530-9, HP-SIS, Done, RUSH. Round 2: Sinering TaC coating
|
John Wong wrote:
|
Monday, September 26, 2016, 13:49, Laura Lambert, SiC, 39530-9, HP-FEBIAD, Done, Sintering SiC#35
|
John Wong wrote:
|
Wednesday, September 28, 2016, 17:09, Laura Lambert, Empty, 41790-6, LP-SIS, Done, sintering TaC coating on UCx container
|
Wednesday, September 28, 2016, 17:08
Container coated with TaC using 'flushing technique' today, cleaned ionizer tube with acetone,
no coating inside ionizer tube |
Thursday, October 13, 2016, 17:32, Laura Lambert, Ta, 41790-5, LP-SIS, Done, Conditioning Ta#50
|
John Wong wrote:
|
Tuesday, October 18, 2016, 09:23, Laura Lambert, Ta, 41790-5, LP-SIS, Done, Temperature measurements for Ta#50
|
Aurelia Laxdal wrote:
|
Monday, October 24, 2016, 17:52, John Wong, np-SiC, , TARGET BOAT, Done, Thermo test of np-SiC raw powder
|
Monday, October 24, 2016, 17:43
Two samples were prepared and loaded into the target boat with 1 layer of heat-shied as shown in the attachment#1.
Ingredients used: np-SiC and very small about of 5% PVA to hold the powder together. |
Friday, November 18, 2016, 17:28, John Wong, np-SiC, , TARGET BOAT, Done, Heat-treatment: Beta-SiC (1um) fiber mats - SAMPLE ID: A1
|
Laura Lambert wrote:
|
Tuesday, November 22, 2016, 15:58, Laura Lambert, Nb, 40282-3, TARGET BOAT, Done, Conditioning Nb samples for Doug
|
Tuesday, November 22, 2016, 15:53
Target boat has a layer of niobium foil on the bottom of the boat.
A niobium foil has been made with slots to hold samples [similar to when sintering endcaps] *See |
|