Thursday, October 02, 2014, 11:52, Laura Lambert, Empty, 40282-5, LP-SIS, In progress, Sintering TaC coating container for UCx#11
|
Thursday, October 02, 2014, 11:51
Target container sprayed with TaC, currently drying in fume hood
Monday, October 06, 2014, 12:11 |
Thursday, September 24, 2015, 09:48, Laura Lambert, Empty, 41077-5, , In progress, Sintering TaC coating container for UCx Target
|
Thursday, September 24, 2015, 08:39
IGP1 = 6.5e-7Torr
HS water valves opened, no leaks detected. |
Thursday, September 24, 2015, 12:18, John Wong, Empty, 41077-5, LP-SIS, Done, Sintering TaC coating container for UCx Target
|
Laura Lambert wrote:
Thursday, September 24, 2015, 08:39 |
Thursday, June 04, 2015, 11:10, Laura Lambert, Empty, , LP-IG-LIS, In progress, Sintering TaC coating container for UCx
|
Thursday, June 04, 2015, 9:07
Container was sprayed with TaC and let dry.
Container has 3x Ta heat shields including center block. |
Friday, June 05, 2015, 12:19, John Wong, Empty, , LP-IG-LIS, In progress, Sintering TaC coating container for UCx
|
Laura Lambert wrote:
Thursday, June 04, 2015, 9:07 |
Friday, June 05, 2015, 13:22, Laura Lambert, Empty, 40860-1, LP-IG-LIS, In progress, Sintering TaC coating container for UCx
|
John Wong wrote:
|
Wednesday, June 10, 2015, 12:15, John Wong, Empty, 40860-1, LP-IG-LIS, In progress, Sintering TaC coating container for UCx
|
Laura Lambert wrote:
|
Friday, June 12, 2015, 14:59, Laura Lambert, Empty, 40860-1, LP-IG-LIS, In progress, Sintering TaC coating container for UCx
|
John Wong wrote:
|
Tuesday, February 11, 2014, 13:49, Laura Lambert, Empty, 38817-8, HP-SIS, Done, Sintering TaC coating container for TiC
|
Tuesday, February 11, 2014, 13:43
Target container is coated with TaC and wrapped with 3-Ta heat shields.
TGHT and TBHT will be ramped up to 820A and 300A, respectively. |
Friday, January 31, 2014, 12:10, Laura Lambert, Empty, 39165-10, LP-SIS, Done, Sintering TaC coating container for Ta?
|
Friday, January 31, 2014, 11:28
Target container is coated with TaC.
The container is wrapped with 3 x Ta heat-shield. |
Thursday, April 09, 2015, 09:38, Laura Lambert, Empty, 38817-7, HP-SIS, Done, Sintering TaC coating container for SiC#32
|
Thursday, April 09, 2015, 09:33
Target container is coated with TaC and wrapped with 3-Ta heat shields, not incl center block.
TGHT and TBHT will be ramped up to 820A and 230A, respectively. |
Tuesday, June 17, 2014, 13:20, Laura Lambert, Empty, 39530-8, HP-FEBIAD, Done, Sintering TaC coating container for SiC#30 part 2
|
Tuesday, June 17, 2014, 13:11
Target container is coated with TaC.
Container is wrapped with 3x Ta-heat shields. |
Wednesday, September 07, 2016, 15:02, John Wong, Empty, 39530-9, HP-SIS, In progress, Sintering TaC coating container for SiC Target
|
Wednesday, September 07, 2016, 14:45
Container was previously coated with TaC solution and wrapped with 1-full length layer of Ta- heat shield around the fins.
Chamber is being pumped down. Vac at 5.6e-7 Torr before HS water valves were open; no leaks were detected. |
Tuesday, August 25, 2015, 11:54, Laura Lambert, Empty, , HP-FEBIAD, In progress, Sintering TaC coating container for SiC Target
|
Tuesday, August 25, 2015, 11:50
Container coated with TaC using new method: Ends tapped off, with liquid poured in and swirled around entire container, then poured back
out - 'flushing technique' |
Thursday, August 27, 2015, 16:37, John Wong, Empty, , HP-FEBIAD, Done, Sintering TaC coating container for SiC Target
|
Laura Lambert wrote:
Tuesday, August 25, 2015, 11:50 |
Thursday, January 16, 2014, 13:06, Laura Lambert, Empty, 39165-9, LP-SIS, In progress, Sintering TaC coating container
|
John Wong wrote:
Wednesday, January 15, 2014, 17:30 |
Friday, January 17, 2014, 09:34, John Wong, Empty, 39165-9, LP-SIS, In progress, Sintering TaC coating container
|
Laura Lambert wrote:
|
Friday, January 17, 2014, 12:52, John Wong, Empty, 39165-9, LP-SIS, In progress, Sintering TaC coating container
|
Laura Lambert wrote:
|
Monday, January 20, 2014, 16:30, Laura Lambert, Empty, 39165-9, LP-SIS, Done, Sintering TaC coating container
|
John Wong wrote:
|
Wednesday, January 15, 2014, 17:45, John Wong, Empty, 39165-9, LP-SIS, In progress, Sintering TaC coating container
|
Wednesday, January 15, 2014, 17:30
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min. |
|