Tuesday, December 01, 2015, 11:35, Anders Mjos, Empty, 41077-5, LP-SIS, In progress, Test#2: Measuring temp with thermocouple (away from centre) & 2C-IR
|
Data from thermocouple attached. Raw data and Excel sheet with plot. |
Wednesday, October 21, 2015, 17:39, John Wong, Empty, 41077-3, LP-SIS, In progress, Sintering TaC on LPSIS (small block) container
|
Wednesday, October 21, 2015, 17:35
This container is prepared for a backup UCx target (otherwise it will be used for development purposes).
The container is coated with TaC; one layer of Ta-heat shield is used. |
Thursday, October 22, 2015, 11:41, Laura Lambert, Empty, 41077-3, LP-SIS, In progress, Sintering TaC on LPSIS (small block) container
|
John Wong wrote:
Wednesday, October 21, 2015, 17:35 |
Thursday, October 22, 2015, 17:10, John Wong, Empty, 41077-3, LP-SIS, In progress, Sintering TaC on LPSIS (small block) container
|
Laura Lambert wrote:
|
Monday, October 26, 2015, 16:14, Laura Lambert, Empty, 41077-3, LP-SIS, Done, Sintering TaC on LPSIS (small block) container & temp measurements with 1xTa h.s
|
John Wong wrote:
|
Monday, October 26, 2015, 16:17, Laura Lambert, Empty, 41077-3, LP-SIS, Done, temp measurements with 2xTa h.s on LPSIS (small block) container 6x
|
Monday, October 26, 2015, 16:16
Container previously sintered with TaC coating and temperature measurements taken with 1x Ta heat shield [see elog ID# 256]
2x Ta heat shields on this container. |
Monday, November 02, 2015, 16:29, Laura Lambert, Empty, 41077-3, LP-SIS, Done, temp measurements with 3xTa h.s on LPSIS (small block) container
|
Monday, November 02, 2015, 16:28
Container previously sintered with TaC coating and temperature measurements taken with 1x Ta
heat shield [see elog ID# 256] and 2x Ta heat shield [see elog ID#257] |
Thursday, November 05, 2015, 16:20, Laura Lambert, , 41077-3, LP-SIS, In progress, Sintering TaC coating on 'temporary endcaps' springs
|
Thursday, November 05, 2015, 16:19
Springs coated with TaC and loaded into container for sintering.
3x Ta heat shield. |
Monday, November 09, 2015, 12:56, John Wong, , 41077-3, LP-SIS, In progress, Sintering TaC coating on 'temporary endcaps' springs (Slope changed to 1.04)
|
Laura Lambert wrote:
Thursday, November 05, 2015, 16:19 |
Monday, November 09, 2015, 14:22, Laura Lambert, , 41077-3, LP-SIS, Done, Sintering TaC coating on 'temporary endcaps' springs (Slope changed to 1.04)
|
John Wong wrote:
|
Tuesday, November 10, 2015, 14:34, Laura Lambert, SiC, 41077-3, LP-SIS, Done, temp measurements with 3xTa h.s on LPSIS (small block) container with SiC
|
Tuesday, November 10, 2015, 14:20
Container previously sintered with TaC coating and temperature measurements taken [see elog ID#
256, 257, 258] |
Monday, January 11, 2016, 15:47, Laura Lambert, SiC, 41077-3, LP-SIS, Done, Conditioning SiC test target for test stand measurements
|
Monday, January 11, 2016, 15:25
Small center block LP-SIS container previously sintered with TaC coating
3x Ta heat shields |
Monday, February 02, 2015, 16:33, John Wong, Empty, 41077-2, LP-SIS, In progress, Coating/Sintering TaC on target container - For Graphite Insert
|
Monday, February 02, 2015, 16:28
Container is coated with TaC. No Ta foil wrapped around.
Chamber is being pumped down. |
Tuesday, February 03, 2015, 10:31, Laura Lambert, Empty, 41077-2, LP-SIS, In progress, Coating/Sintering TaC on target container - For Graphite Insert
|
John Wong wrote:
Monday, February 02, 2015, 16:28 |
Thursday, February 05, 2015, 18:03, John Wong, Empty, 41077-2, LP-SIS, In progress, Coating/Sintering TaC on target container - For Graphite Insert
|
Laura Lambert wrote:
|
Tuesday, February 10, 2015, 13:19, Laura Lambert, Empty, 41077-2, LP-SIS, Done, Coating/Sintering TaC on target container - For Graphite Insert
|
John Wong wrote:
|
Tuesday, February 10, 2015, 14:01, Laura Lambert, Empty, 41077-2, LP-SIS, Done, Conditioning graphite insert inside container - no heat shield
|
Tuesday, February 10, 2015, 14:00
Container loaded into EVAP2 at noon.
no heat shields. |
Wednesday, February 11, 2015, 16:12, Laura Lambert, Empty, 41077-2, LP-SIS, Done, Conditioning graphite insert inside container - with heat shield
|
Wednesday, February 11, 2015, 16:10
Container loaded into EVAP2.
3xTa heat shields. |
Friday, February 12, 2016, 11:09, Laura Lambert, Empty, 41077-1, LP-SIS, Done, sintering TaC coated small center block container
|
Friday, February 12, 2016, 11:01
Container coated with TaC with new method - ends tapped off, liquid poured/swirled
around container, then poured back out - 'flushing technique'. |
Friday, July 15, 2016, 11:52, Laura Lambert, Empty, 40860-3, LP-IG-LIS, Done, sintering TaC coating on SiC#34 container
|
Friday, July 15, 2016, 11:49
Container previously coated with TaC using 'flushing technique', cleaned ionizer tube with acetone,
so no coating inside ionizer tube |
|