Thursday, July 12, 2012, 17:55, John Wong, NiO, targetboat (TaC coated), , Maintenance, NiO development- test#2
|
Thursday, July 12, 2012, 17:29
NiO was sprayed on Ni foil.
Average/discs: mass= 0.075g, thickness=0.076mm, density = 7.023g/cm3. |
Tuesday, July 17, 2012, 16:00, John Wong, , targetboat (TaC coated), , Done, Sintering TaC coated regular- & D-endcaps
|
Tuesday, July 17, 2012, 15:45
Target boat is filled with TaC coated regular- and D-endcaps.
The boat is wrapped with a Ta heat-shield. |
Tuesday, August 27, 2013, 17:01, John Wong, , targetboat (TaC coated), , Done, Sintering TaC coated regular caps
|
Tuesday, August 27, 2013, 16:48
Target boat is filled with TaC coated endcaps (brown) and some partial sinterred ones (gray) from before. (see attachment#1).
The container is wrapped with Ta heat-shield. |
Thursday, August 29, 2013, 11:53, Laura Lambert, , targetboat (TaC coated), , Done, Sintering TaC coated regular caps
|
John Wong wrote:
Tuesday, August 27, 2013, 16:48 |
Tuesday, January 19, 2016, 14:27, John Wong, np-SiC, targetboat (TaC coated), TARGET BOAT, Done, SiC Nanofiber Heat Treatment
|
Tuesday, January 19, 2016, 14:19
SiC nanofiber was prepared at UBC Material Engineering Sci.
4 samples are loaded in a Ta target contained (sintered with TaC coating): |
Tuesday, September 17, 2013, 11:21, John Wong, Nb, target boat #3 (brand new!) , , , Nb thermo treatment (Bob's samples)
|
Tuesday, September 17, 2013, 11:14
Target boat contains 5 Nb discs. 3 discs are wraps with 0.001" thin of Nb foil (99.8% pure), and 2 are wraps with 0.001" Ta foil
(see attachment#1) |
Thursday, September 19, 2013, 11:56, Laura Lambert, Nb, target boat #3 (brand new!) , , , Nb thermo treatment (Bob's samples)
|
John Wong wrote:
Tuesday, September 17, 2013, 11:14 |
Thursday, September 19, 2013, 17:02, John Wong, Nb, target boat #3 (brand new!) , , , Nb thermo treatment (Bob's samples)
|
Laura Lambert wrote:
|
Friday, September 20, 2013, 14:59, John Wong, Nb, target boat #3 (brand new!) , , , Nb thermo treatment (Bob's samples)
|
John Wong wrote:
Tuesday, September 17, 2013, 11:14 |
Monday, September 23, 2013, 16:18, John Wong, Nb, target boat #3 (brand new!) , , , Nb thermo treatment (Bob's samples)
|
John Wong wrote:
|
Friday, February 26, 2021, 09:28, Ferran Boix Pamies, Empty, none, , Done, Parasitic target thermal tests
|
Tests were performed with external power supply. No target boat or container.
Small power on heating small heating elements on parasitic target attached on isac heatshield with water cooling on.
|
Wednesday, June 08, 2022, 10:00, Flora Wu, , boat, , Done, carbonize PAN 10% discs
|
Thursday, June 09, 2022, 11:25
Total number of foils: 14 electrospun fiber pellets
Total weight = 208.3 g |
Thursday, June 09, 2022, 19:20, John Wong, , boat, , Done, carbonize PAN 10% discs
|
Flora Wu wrote:
Thursday, June 09, 2022, 11:25 |
Saturday, April 28, 2018, 16:12, John Wong, Empty, Tube container , , Done, TaC coating/sintering of Tube container
|
Saturday, April 28, 2018, 16:09
Container is coated with TaC and wrapped with TaC heatshield.
Will be used for carbonizing nanoSiC target materials. |
Tuesday, May 08, 2018, 15:06, John Wong, np-SiC, Tube container , , Done, NanoSiC thermal treatment batch#2
|
Tuesday, May 08, 2018, 15:02
22 np-SiC fibrous discs loaded in the tube container (coated and sintered with TaC)
Heat treatment is similar to previous process, see elog #408. |
Tuesday, May 01, 2018, 18:07, John Wong, np-SiC, Tube container, , Done, NanoSiC thermal treatment batch#1
|
Tuesday, May 01, 2018, 18:06
21 fibrous discs of nanoSiC are loaded into a tube container (coated/Sintered with TaC).
Thermal treatment temperature at 1600C, TGHT is ~338A/5.5V, according to elog #407. |
Tuesday, July 03, 2018, 17:05, John Wong, np-SiC, Tube container, , Done, NanoSiC thermal treatment batch #3
|
Tuesday, July 03, 2018, 17:02
49 discs/ 15.42g np-SiC fibrous discs loaded into the tube container
Heat treatment is similar to previous process, see elog#408/409. |
Tuesday, February 28, 2012, 11:00, John Wong, Empty, Test oven , LP-SIS, Done, Measuring temperatures, currents & voltages
|
Tuesday, February 28, 2012, 10:36
Two thermocouples were inserted through the left side of the copper heat shield, see attachment #1. One thermocouple is attached to the target
tube with a Ta-wire, and the other is attached to the back block. |
Tuesday, October 18, 2022, 13:59, Hannah Toy, TiC, Target boat (tube), TARGET BOAT, Done, Synthesis of TiC
|
Tuesday, October 18, 2022, 13:52
38 pieces of samples made of TiO2/C/PVP loaded into a target boat wrapped with 2 layers of Ta-heat shield.
Samples will be heated to 1700, 1800, 1900, and 2000 C |
Wednesday, October 19, 2022, 09:50, John Wong, TiC, Target boat (tube), TARGET BOAT, Done, Synthesis of TiC
|
Hannah Toy wrote:
Tuesday, October 18, 2022, 13:52 |
|