Logbooks Lab Maintenance Evaporator_1 Evaporator_2 Laser cutter Target Production Test-Stand RH-ISAC RH-Cyclotron RH-Meson Hall RH-Beamlines RH-ARIEL
  Evaporator_2, Page 16 of 25  Not logged in ELOG logo
Entry  Thursday, February 09, 2017, 11:49, Laura Lambert, , , , Maintenance, New heatshield with flexible water lines 
 Thursday, February 09, 2017, 11:47
A new heatshield with flexible water lines has been put into evap2 last Friday Feb3rd

 
Entry  Monday, February 06, 2017, 11:17, Anders Mjos, , , , Problems resolved, IOC restart after power outagae 
 Dave Morris did a remote restart of the IOC after the outage. Turbo pump started.
Entry  Tuesday, January 31, 2017, 16:03, Laura Lambert, Empty, 39530-10, HP-FEBIAD, Done, Sintering TaC coated container for backup 39530-10(1).JPG39530-10(2).JPG
 Tuesday, January 31, 2017, 13:43
Container coated with TaC using new method: Ends taped off,  with liquid poured in and swirled
around entire container, then poured back out - 'flushing technique'
Entry  Tuesday, December 20, 2016, 15:04, Laura Lambert, , , , Maintenance, RETURN and SUPPLY valves CLOSED for xmas break 
Tuesday, December 20, 2016, 15:05
confirmed ~full tank of Ar for glove box --> ~1600psi 
Entry  Friday, December 16, 2016, 14:14, Laura Lambert, Ta, 39530-3, LP-FEBIAD, Done, Conditioning Ta FEBIAD target for shutdown tests Ta-FEBIAD.xlsxEvernote_Camera_Roll_20161220_145947.jpg
 Friday, December 16, 2016, 14:08
Target consists of 470 discs.
Total packed length 3.4cm [exactly 7.8cm space on both sides]
Entry  Thursday, December 01, 2016, 16:08, Laura Lambert, Empty, 42218-12, LP-SIS, Done, sintering TaC coating on UCx#19 container 
 Thursday, December 01, 2016, 16:06
Container coated with TaC using 'flushing technique' and let dry overnight.
Cleaned ionizer tube with acetone, no coating inside ionizer tube
Entry  Tuesday, November 22, 2016, 15:58, Laura Lambert, Nb, 40282-3, TARGET BOAT, Done, Conditioning Nb samples for Doug samples.jpgevap2.jpgheating_up.xlsxvisual_of_MIKRON_pointing_at_samples.JPG
Tuesday, November 22, 2016, 15:53
Target boat has a layer of niobium foil on the bottom of the boat.
A niobium foil has been made with slots to hold samples [similar to when sintering endcaps] *See
Entry  Tuesday, November 15, 2016, 16:51, John Wong, np-SiC, , TARGET BOAT, In progress, Heat-treatment: Beta-SiC (1um) fiber mats - SAMPLE ID: A1 
Tuesday, November 15, 2016, 16:48
Three samples were prepared  (see my logbook#1 page 3, preparing for carbonization).
One layer of Ta foil was used to wrap around the target boat. 
    Reply  Thursday, November 17, 2016, 11:15, Laura Lambert, np-SiC, , TARGET BOAT, In progress, Heat-treatment: Beta-SiC (1um) fiber mats - SAMPLE ID: A1 


    
        
            John Wong wrote:
        
        
            
            Tuesday, November 15, 2016, 16:48
       Reply  Friday, November 18, 2016, 17:28, John Wong, np-SiC, , TARGET BOAT, Done, Heat-treatment: Beta-SiC (1um) fiber mats - SAMPLE ID: A1 


    
        
            Laura Lambert wrote:
        
        
            
            
            
Entry  Monday, October 24, 2016, 17:52, John Wong, np-SiC, , TARGET BOAT, Done, Thermo test of np-SiC raw powder  Capture.JPG450A_1500C.JPG
Monday, October 24, 2016, 17:43
Two samples were prepared and loaded into the target boat with 1 layer of heat-shied as shown in the attachment#1.
Ingredients used: np-SiC and very small about of 5% PVA to hold the powder together. 
Entry  Thursday, October 13, 2016, 18:05, Laura Lambert, Ta, 41790-5, LP-SIS, In progress, Temperature measurements for Ta#50 
Thursday, October 13, 2016, 18:04
Target loaded into evap2
No heat shields.
    Reply  Saturday, October 15, 2016, 12:42, Aurelia Laxdal, Ta, 41790-5, LP-SIS, In progress, Temperature measurements for Ta#50 


    
        
            Laura Lambert wrote:
        
        
            
            Thursday, October 13, 2016, 18:04
       Reply  Sunday, October 16, 2016, 17:55, Aurelia Laxdal, Ta, 41790-5, LP-SIS, In progress, Temperature measurements for Ta#50 


    
        
            Aurelia Laxdal wrote:
        
        
            
            
            
              
          Reply  Tuesday, October 18, 2016, 09:23, Laura Lambert, Ta, 41790-5, LP-SIS, Done, Temperature measurements for Ta#50 


    
        
            Aurelia Laxdal wrote:
        
        
            
            
            
Entry  Friday, October 07, 2016, 16:42, Laura Lambert, Ta, 41790-5, LP-SIS, In progress, Conditioning Ta#50 Ta#50_no_endcaps_3xh.s..xlsx
Friday, October 07, 2016, 16:40
Target consists of 470 discs.
Total packed length 3.4cm [exactly 7.8cm space on both sides]
    Reply  Wednesday, October 12, 2016, 21:18, John Wong, Ta, 41790-5, LP-SIS, In progress, Conditioning Ta#50 


    
        
            Laura Lambert wrote:
        
        
            
            Friday, October 07, 2016, 16:40
       Reply  Thursday, October 13, 2016, 17:32, Laura Lambert, Ta, 41790-5, LP-SIS, Done, Conditioning Ta#50 


    
        
            John Wong wrote:
        
        
            
            
            
Entry  Wednesday, September 28, 2016, 17:09, Laura Lambert, Empty, 41790-6, LP-SIS, Done, sintering TaC coating on UCx container sintering_TaC_coating.xlsxsintering_TaC_coating.JPGsintering_TaC_coating2.JPGsintering_TaC_coating-combo_of_both_pics.JPG
 Wednesday, September 28, 2016, 17:08
Container coated with TaC using 'flushing technique' today, cleaned ionizer tube with acetone,
no coating inside ionizer tube
Entry  Thursday, September 15, 2016, 16:37, Laura Lambert, SiC, 39530-9, HP-FEBIAD, In progress, Sintering SiC#35 
 Thursday, September 15, 2016, 16:23
Target container contains 487 discs of SiC 
Target packed length = 16cm. 
    Reply  Monday, September 19, 2016, 18:48, John Wong, SiC, 39530-9, HP-FEBIAD, In progress, Sintering SiC#35 - Change OMEGA/MiKRON slopes 


    
        
            Laura Lambert wrote:
        
        
            
             Thursday, September 15, 2016, 16:23
       Reply  Tuesday, September 20, 2016, 15:40, Laura Lambert, SiC, 39530-9, HP-FEBIAD, In progress, Sintering SiC#35 sintering_target_data.xlsx


    
        
            John Wong wrote:
        
        
            
            
            
          Reply  Thursday, September 22, 2016, 12:14, John Wong, SiC, 39530-9, HP-FEBIAD, In progress, Sintering SiC#35 


    
        
            Laura Lambert wrote:
        
        
            
            
            
             Reply  Monday, September 26, 2016, 13:49, Laura Lambert, SiC, 39530-9, HP-FEBIAD, Done, Sintering SiC#35 comparison_of_temperature_drop_-_3x_snapshots.JPG


    
        
            John Wong wrote:
        
        
            
            
            
Entry  Wednesday, September 07, 2016, 15:02, John Wong, Empty, 39530-9, HP-SIS, In progress, Sintering TaC coating container for SiC Target  coating_chipped_off.JPGautoTaC_sintering_20.JPEGcoating_chipped_off_2.JPG
 Wednesday, September 07, 2016, 14:45
Container was previously coated with TaC solution and wrapped with 1-full length layer of Ta- heat shield around the fins.  
Chamber is being pumped down.  Vac at 5.6e-7 Torr before HS water valves were open; no leaks were detected. 
    Reply  Monday, September 12, 2016, 17:22, John Wong, Empty, 39530-9, HP-SIS, Failed, TaC coating chipped off Screen_Shot_2016-09-12_at_4.52.53_PM.png


    
        
            John Wong wrote:
        
        
            
             Wednesday, September 07, 2016, 14:45
       Reply  Monday, September 12, 2016, 17:27, John Wong, Empty, 39530-9, HP-SIS, Done, RUSH. Round 2: Sinering TaC coating  Screen_Shot_2016-09-14_at_5.05.08_PM.pngScreen_Shot_2016-09-14_at_5.03.48_PM.png


    
        
            John Wong wrote:
        
        
            
            
            
Entry  Monday, August 08, 2016, 15:22, Laura Lambert, SiC, 40860-3, LP-IG-LIS, Problems, Conditioning SiC#34 conditioning_temperature_graph.xlsxstriptool_conditioning_target_BROKEN.JPG
 Monday, August 08, 2016, 15:19
Previously sintered over weekend [see elog i.d 311]
Target container contains 471 discs of SiC [6 x 5 packs + 441 single discs]
    Reply  Tuesday, August 30, 2016, 15:25, John Wong, SiC, 40860-3, LP-IG-LIS, Problems, Conditioning SiC#34. Note about the p/s voltage Capture.PNG


    
        
            Laura Lambert wrote:
        
        
            
             Monday, August 08, 2016, 15:19
Entry  Wednesday, August 24, 2016, 17:07, John Wong, SiC, 39814-V2-1, LP-IG-LIS, Done, Sintering process for SiC#34 (2nd round)  10x
Wednesday, August 24, 2016, 17:05
Target container was previously coated with TaC and sintered up to 1900C at 420A/7.01V
Container is loaded with beta-SiC 432 discs at 16cm in length. 
Entry  Wednesday, August 17, 2016, 17:31, Laura Lambert, Empty, 39814-V2-1, LP-IG-LIS, In progress, sintering TaC coating on SiC#34 container...round2 leak.JPGwater_leak.JPEG
 Wednesday, August 17, 2016, 17:30
Container coated with TaC using 'flushing technique', cleaned ionizer tube with acetone, so no
coating inside ionizer tube
    Reply  Tuesday, August 23, 2016, 12:15, John Wong, Empty, 39814-V2-1, LP-IG-LIS, Done, sintering TaC coating on SiC#34 container...round2 


    
        
            Laura Lambert wrote:
        
        
            
             Wednesday, August 17, 2016, 17:30
Entry  Thursday, August 18, 2016, 10:37, Anders Mjos, , , , Maintenance, New cooling lines for Heat Shield 
 Dan made a set of new cooling lines for the Source Tray Heat Shield cooling yesterday. No joints on the lines. Use same VCR fitting 3/8 -> 1/4"
as for the Heat Shield. The old lines had worn threads on the male VCR nut.
Entry  Friday, August 12, 2016, 11:08, Laura Lambert, , , , Maintenance, NEW PUMP FOR GLOVE BOX 
Wednesday, August 03, 2016, 16:16
Tues July 26th had some problems with the transfer chamber
Transfer chamber was not going below -20in pressure, when usually it will drop all the way to -30in
Entry  Tuesday, August 02, 2016, 13:56, Laura Lambert, SiC, 40860-3, LP-IG-LIS, Done, Sintering SiC#34 sintering-_coating_on_window1.jpgsintering-_coating_on_window2.jpgsintering-_coating_on_window3.jpeg
 Tuesday, August 02, 2016, 13:41
Target container contains 471 discs of SiC [6 x 5 packs + 441 single discs]
Target packed length = 16cm. 
ELOG V2.9.2-2455