Thursday, April 11, 2013, 14:20, John Wong, Empty, 39165-6, LP-SIS, Done, Coating target oven /w TaC & sintering for UCx#6
|
Monday, April 08, 2013, 17:39
Target container is coated with TaC; the container will be used for the UCx#6 target.
No Ta-heat shields are used. |
Monday, July 22, 2013, 15:03, John Wong, Empty, 38634-7, LP-SIS, Done, Sintering empty target oven coated with TaC for UCx#7
|
Monday, July 22, 2013, 15:00
Target container is coated with TaC - this container will be used for UCx#7.
Container is wrapped with 3 layers of Ta, including the back-block. |
Friday, October 04, 2013, 16:21, John Wong, Empty, , LP-SIS, Done, Sintering TaC coating on a LP target container to be used for C-grv tube test
|
Friday, October 04, 2013, 15:37
A LP target container is coated with TaC. The container is wrapped with 3 layers to heat shield.
This container will be used for the graphite tube test. |
Wednesday, January 15, 2014, 17:45, John Wong, Empty, 39165-9, LP-SIS, In progress, Sintering TaC coating container
|
Wednesday, January 15, 2014, 17:30
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min. |
Thursday, January 16, 2014, 13:06, Laura Lambert, Empty, 39165-9, LP-SIS, In progress, Sintering TaC coating container
|
John Wong wrote:
Wednesday, January 15, 2014, 17:30 |
Friday, January 17, 2014, 09:34, John Wong, Empty, 39165-9, LP-SIS, In progress, Sintering TaC coating container
|
Laura Lambert wrote:
|
Friday, January 17, 2014, 10:18, Laura Lambert, Empty, 39165-9, LP-SIS, In progress, Sintering TaC coating container
|
John Wong wrote:
|
Friday, January 17, 2014, 12:52, John Wong, Empty, 39165-9, LP-SIS, In progress, Sintering TaC coating container
|
Laura Lambert wrote:
|
Monday, January 20, 2014, 16:30, Laura Lambert, Empty, 39165-9, LP-SIS, Done, Sintering TaC coating container
|
John Wong wrote:
|
Friday, January 31, 2014, 12:10, Laura Lambert, Empty, 39165-10, LP-SIS, Done, Sintering TaC coating container for Ta?
|
Friday, January 31, 2014, 11:28
Target container is coated with TaC.
The container is wrapped with 3 x Ta heat-shield. |
Friday, June 13, 2014, 14:57, Laura Lambert, Ta, 40282-2, LP-SIS, In progress, Conditioning Ta#43 target
|
Friday, June 13, 2014, 14:53
Container is filled with 400 discs of Ta foils; target length = 5.2cm;
Total mass ( Ta foils + wire) = 45.92g |
Monday, June 16, 2014, 17:42, John Wong, Ta, 40282-2, LP-SIS, In progress, Conditioning Ta#43 target
|
Laura Lambert wrote:
Friday, June 13, 2014, 14:53 |
Tuesday, June 17, 2014, 10:14, Laura Lambert, Ta, 40282-2, LP-SIS, Done, Conditioning Ta#43 target
|
John Wong wrote:
|
Wednesday, July 23, 2014, 15:07, John Wong, Empty, 40282-3, LP-SIS, In progress, Sintering TaC coated target container
|
Wednesday, July 23, 2014, 15:07
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min. |
Monday, July 28, 2014, 10:52, Laura Lambert, Empty, 40282-3, LP-SIS, Done, Sintering TaC coated target container
|
John Wong wrote:
Wednesday, July 23, 2014, 15:07 |
Monday, July 28, 2014, 15:06, Laura Lambert, , 40282-3, LP-SIS, In progress, Sintering ZrC# 6 target
|
Monday, July 28, 2014, 14:41
Total number of foils: 445 discs
Total mass of materials [incl graphite foils]: 49.027 g |
Tuesday, July 29, 2014, 11:23, John Wong, , 40282-3, LP-SIS, In progress, Sintering ZrC# 6 target
|
Laura Lambert wrote:
Monday, July 28, 2014, 14:41 |
Friday, August 01, 2014, 11:47, Peter Kunz , , 40282-3, LP-SIS, In progress, ZrC #6 conditioning
|
The maximum current of 580A was reached at 9:15.
TGHT:RDCUR 578 A
TGHT:RDVOL 9.87 V |
Friday, August 01, 2014, 13:27, Peter Kunz , , 40282-3, LP-SIS, In progress, ZrC #6 conditioning
|
Target was conditioned for 4 hours at 580A.
Initiating ramp-down sequence @ 2A/min
|
Tuesday, August 05, 2014, 12:01, Laura Lambert, , 40282-3, LP-SIS, Done, ZrC #6 conditioning
|
Peter Kunz wrote:
Target was conditioned for 4 hours at 580A. |
|