ID |
Date |
Author |
Target Material |
Target Oven W.O# |
Source |
Status |
Subject |
Text |
 |
|
209
|
Friday, June 05, 2015, 13:22 |
Laura Lambert | Empty | 40860-1 | LP-IG-LIS | In progress | Sintering TaC coating container for UCx |
|
 |
|
208
|
Friday, June 05, 2015, 12:19 |
John Wong | Empty | | LP-IG-LIS | In progress | Sintering TaC coating container for UCx |
|
|
|
207
|
Thursday, June 04, 2015, 11:10 |
Laura Lambert | Empty | | LP-IG-LIS | In progress | Sintering TaC coating container for UCx | Thursday, June 04, 2015, 9:07
Container was sprayed with TaC and
let dry. |
|
|
206
|
Wednesday, June 03, 2015, 10:47 |
Laura Lambert | ZrC | 41177-1 | LP-SIS | Done | Conditioning ZrC#7 |
|
|
|
205
|
Tuesday, June 02, 2015, 13:05 |
John Wong | ZrC | 41177-1 | LP-SIS | Done | Conditioning ZrC#7 |
|
|
|
204
|
Monday, June 01, 2015, 18:09 |
John Wong | ZrC | 41177-1 | LP-SIS | In progress | Conditioning ZrC#7 |
|
|
|
203
|
Friday, May 29, 2015, 11:29 |
Laura Lambert | ZrC | 41177-1 | LP-SIS | In progress | Conditioning ZrC#7 | Friday, May 29, 2015, 11:21
Total number of foils: 425 discs |
|
|
202
|
Friday, May 29, 2015, 11:18 |
Laura Lambert | Endcaps | 40282-5 | TARGET BOAT | Done | Sintering TaC coating on Ta endcaps - round 2 |
|
 |
|
201
|
Thursday, May 28, 2015, 17:50 |
John Wong | Endcaps | 40282-5 | TARGET BOAT | Done | Sintering TaC coating on Ta endcaps - round 2 |
|
|
|
200
|
Thursday, May 28, 2015, 11:36 |
Laura Lambert | Endcaps | 40282-5 | TARGET BOAT | In progress | Sintering TaC coating on Ta endcaps - round 2 | Thursday, May 28, 2015, 11:34
Endcaps were sintered [see elog#199] |
|
|
199
|
Thursday, May 28, 2015, 10:23 |
Laura Lambert | Endcaps | 40282-5 | TARGET BOAT | Problems | Sintering TaC coating on Ta endcaps - not fully sintered |
|
 |
|
198
|
Wednesday, May 27, 2015, 17:58 |
John Wong | Endcaps | 40282-5 | TARGET BOAT | In progress | Sintering TaC coating on Ta endcaps |
|
|
|
197
|
Tuesday, May 26, 2015, 13:57 |
Laura Lambert | Endcaps | 40282-5 | TARGET BOAT | In progress | Sintering TaC coating on Ta endcaps | Tuesday, May 26, 2015, 13:06
Endcaps were sprayed with TaC coating
and let dry. |
|
|
196
|
Tuesday, May 26, 2015, 13:05 |
Laura Lambert | Empty | 40282-5 | TARGET BOAT | Done | Sintering TaC coating on Ta target boat |
|
|
|
195
|
Monday, May 25, 2015, 17:08 |
John Wong | Empty | 40282-5 | TARGET BOAT | In progress | Sintering TaC coating on Ta target boat |
|
|
|
194
|
Friday, May 22, 2015, 11:44 |
Laura Lambert | Empty | | TARGET BOAT | In progress | Sintering TaC coating on Ta target boat | Friday, May 22, 2015, 11:43
A target boat was sprayed with |
|
|
193
|
Tuesday, May 19, 2015, 13:54 |
Laura Lambert | Empty | 41177-1 | LP-SIS | Done | Sintering TaC coating container for ZrC | Tuesday, May 19, 2015, 13:33
Target container is coated with |
|
|
192
|
Wednesday, May 13, 2015, 16:01 |
Laura Lambert | | 40282-4 | TARGET BOAT | Done | Sintering three different ZrC samples | Wednesday, May 13, 2015, 15:21
Three different samples of ZrC |
|
|
191
|
Friday, May 08, 2015, 15:56 |
Laura Lambert | | 40282-4 | TARGET BOAT | Done | Sintering four different ZrC samples |
|
|
|
190
|
Wednesday, May 06, 2015, 13:59 |
Laura Lambert | | 40282-4 | TARGET BOAT | Done | Sintering two different ZrC samples | Wednesday, May 06, 2015, 13:54
Two different samples of ZrC are
wrapped in graphite sheet and loaded into |
|