Monday, November 10, 2014, 13:50, Laura Lambert, UC2, 40282-5, LP-SIS, Done, Conditioning UCx #11
|
John Wong wrote:
|
Monday, January 26, 2015, 11:28, Laura Lambert, UO2/C, 40282-1, TARGET BOAT, Done, Processing UC2Flk_05
|
Monday, January 26, 2015, 11:19
UO2/C green was prepared Jan 20, 2015. The slurry was cast on a piece of glass coated with WD40 on Jan 21, 2015.
The cast was let dry over the weekend and peeled off the glass nicely Jan 26, 2014. [see attached picture] |
Friday, March 20, 2015, 15:21, Laura Lambert, UC2, 41177-2, LP-SIS, Done, Conditioning UCx #12
|
Friday, March 20, 2015, 15:17
Target container was previously coated with TaC spray and sintered.
It's is wrapped with 3 layers of Ta-heat shield, including the center block. |
Monday, May 11, 2015, 11:49, Laura Lambert, UO2/C, 40282-1, TARGET BOAT, Done, Processing UC2Flk_06
|
Monday, May 11, 2015, 11:45
UO2/C green was prepared May 6, 2015. The slurry was cast on a piece of glass coated with WD40
on May 7, 2015. |
Wednesday, July 08, 2015, 10:52, John Wong, UC2, 40860-1, LP-IG-LIS, Done, Conditioning UCx #13
|
Laura Lambert wrote:
|
Tuesday, August 11, 2015, 10:23, Laura Lambert, UO2/C, 40282-1, TARGET BOAT, Done, Processing UC2_flk_07
|
John Wong wrote:
Thursday, July 30, 2015, 17:10 |
Wednesday, August 19, 2015, 11:44, Laura Lambert, UO2/C, 40282-1, TARGET BOAT, Done, Processing UC2Flk_08 8x
|
Wednesday, August 19, 2015, 11:02
UO2/C green was prepared Aug 11, 2015. The slurry was cast on a piece of glass coated with WD40
on Aug 12, 2015. |
Monday, September 14, 2015, 15:31, John Wong, UO2/C, 40282-1, TARGET BOAT, Done, Processing UC2Flk_09
|
Monday, September 14, 2015, 15:28
Green cast dried UO2/C + organic mass = 61.31g
The green was rolled up and wrapped in a piece of graphite sheet. |
Monday, October 26, 2015, 16:20, Laura Lambert, UC2, 41077-5, LP-SIS, Done, Conditioning UCx#14
|
John Wong wrote:
Thursday, October 15, 2015, 15:52 |
Friday, December 04, 2015, 15:06, Laura Lambert, UO2/C, 40282-1, TARGET BOAT, Done, 1stepUCx project - round1
|
Wednesday, December 02, 2015, 14:08
UO2/C was cast onto a graphite sheet in the fume hood and let dry.
Initial UO2 powder used = 25.11g (Inventory R-00835A, UO2 + bottle = 243.44g before use) |
Thursday, December 10, 2015, 10:59, Laura Lambert, UO2/C, 40282-1, TARGET BOAT, Done, 1stepUCx project - round2
|
Thursday, December 10, 2015, 08:54
Filled graphite tube with 34 UO2/C discs cast onto graphite.
34 discs = 4.10g |
Monday, February 29, 2016, 16:16, Laura Lambert, UC2, 41077-1, LP-SIS, Done, Conditioning UCx#15
|
John Wong wrote:
|
Tuesday, March 08, 2016, 11:19, Laura Lambert, UO2/C, 40282-1, TARGET BOAT, Done, Processing UC2Flk_10
|
Tuesday, March 08, 2016, 10:01
UO2/C green was prepared March 2, 2016.
This was the first time using the new rack built for holding multiple casts [see photo attached] |
Tuesday, April 05, 2016, 11:12, Laura Lambert, UO2/C, 40282-1, TARGET BOAT, Done, Processing UC2Flk_11
|
Tuesday, April 05, 2016, 10:58
UO2/C green was prepared March 31, 2016.
The cast peeled off the glass nicely April 1, 2016 and finished drying over the weekend. [see |
Tuesday, April 19, 2016, 10:48, Laura Lambert, UC2, ***, , Done, ***ALL FUTURE UCx TARGETS***
|
Tuesday, April 19, 2016, 09:47
Temperature measurements have been taken in evap2 on target containers.
Previously all UCx targets have been conditioned in evap1 at 520A. The respective target containers TaC coating was sintered in evap2 at a |
Wednesday, May 18, 2016, 15:15, Laura Lambert, UC2, 40860-2, LP-IG-LIS, Done, Conditioning UCx#16
|
Wednesday, May 18, 2016, 15:05
Target container was previously coated with TaC spray and sintered.
Container is wrapped with 3 layers of Ta-heat shield, including the center block - new wrapping |
Monday, July 11, 2016, 16:00, Laura Lambert, UC2, 41790-3, LP-SIS, Done, Conditioning UCx#17
|
Monday, July 11, 2016, 15:54
Target container was previously coated with TaC spray and sintered.
Container is wrapped with 3 layers of Ta-heat shield, including the center block - new wrapping |
Tuesday, September 20, 2016, 10:49, Laura Lambert, , , TARGET BOAT, Done, RUSH. Sintering end-caps
|
John Wong wrote:
Monday, September 12, 2016, 17:30 |
Friday, September 23, 2016, 16:09, Laura Lambert, UO2/C, 40282-1, TARGET BOAT, Done, Processing UC2Flk_12
|
Friday, September 23, 2016, 16:01
*Note: materials were scaled back small amount since only 48.5g of UO2 was left in bottle when usually 50g required to make slurry
UO2/C green was prepared September 22, 2016. |
Wednesday, October 19, 2016, 16:52, Laura Lambert, UC2, 41790-6, LP-SIS, Done, Conditioning UCx#18
|
Wednesday, October 19, 2016, 16:47
Target container was previously coated with TaC spray and sintered.
Container is wrapped with 3 layers of Ta-heat shield, including the center block using one single |
|