Logbooks Lab Maintenance Evaporator_1 Evaporator_2 Laser cutter Target Production Test-Stand RH-ISAC RH-Cyclotron RH-Meson Hall RH-Beamlines RH-ARIEL
  Evaporator_2, Page 16 of 34  Not logged in ELOG logo
Entry  Thursday, April 08, 2021, 08:25, Aaron Schmidt, Ta, 44139-10, LP-SIS, In progress, Conditioning Ta#62 & Flex - line HS installed 
 Ta#62 LP-SIS target description:
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.025mm
Entry  Wednesday, June 23, 2021, 17:48, Aaron Schmidt, Ta, 44691-4, LP-SIS, In progress, Conditioning Ta#62 (Replacement) Ta#62_conditioning_-_Evap_2_-_44691-4.docx
 Ta#62 LP-SIS target description: (REPLACEMENT FOR 44139-10)
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.025mm
Entry  Thursday, August 05, 2021, 11:18, Darwin Ortiz Rosales, SiC, 44691-2, LP-SIS, Done, Dr blade and non-Dr blade Material Experiment (sintering) image_2021-08-09_221014.png
Thursday, August 05, 2021, 11:10
Total number of foils: 380
Total length packed 13.5 cm
Entry  Thursday, September 02, 2021, 07:14, Darwin Ortiz Rosales, TaC, 44691-7, LP-SIS, Done, TaC coating/sintering coating44691-7.PNG
 Thursday, September 02, 2021, 06:36
Ta tube was coated with TaC and wrapped with Ta heat-shields (3 layers)
Desired temperature = 1900 C (expected TGHT ~430 A), TBHT will be set fixed at 230A (max).
Entry  Wednesday, October 27, 2021, 11:09, Darwin Ortiz Rosales, Ta, 44691-3, LP-SIS, Done, TaC coating/sintering 
 Wednesday, October 27, 2021, 11:07
Monday, October 25, 2021, 11:52
Ta LPSIS tube was coated with TaC and wrapped with Ta heat-shields (3 layers)
Entry  Monday, November 01, 2021, 07:39, Darwin Ortiz Rosales, Empty, 44508-3, LP-SIS, Done, TaC coating/sintering 211101-TaC_coating.png
 Monday, November 01, 2021, 07:37
Ta tube was coated with TaC and wrapped with Ta heat-shields (3 layers)
Note* on the leading end of the assembly I placed tantalum foil heatshield similar to what I
Entry  Wednesday, November 03, 2021, 09:24, Darwin Ortiz Rosales, Empty, 44691-10, LP-SIS, Done, TaC coating/sintering 
 Ta tube was coated with TaC and wrapped with Ta heat-shields (3 layers)
Note:  placed tantalum foil heatshield on both sides of the copper heatshield assembly.
Desired temperature = 1800 C (expected TGHT ~430 A), TBHT will be set fixed at 230A (max).
Entry  Wednesday, November 10, 2021, 18:07, Aaron Schmidt, Ta, 44691-11, LP-SIS, In progress, Conditioning Ta#63 
Ta#63 LP-SIS target description: 
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.025mm
Entry  Thursday, June 02, 2022, 16:53, Aaron Schmidt, Ta, 44691-12, LP-SIS, In progress, Conditioning Ta#64 
 Ta#64 LP-SIS target description: 
Total Ta foils = 470 [6x20 packs + 350 single discs]
Foil Thickness = 0.0254mm (0.0010") Measured.
Entry  Thursday, September 01, 2022, 12:32, Darwin Ortiz Rosales, TaC, 44691-13, LP-SIS, Done, TaC coating sintering MicrosoftTeams-image_(13).png
Thursday, September 01, 2022, 10:34
The coated container was wrapped in three Ta foil heatshields.
Target temperature on OMEGA= 1850-1900 C
Entry  Monday, October 17, 2022, 11:32, Darwin Ortiz Rosales, TaC, 45220-2, LP-SIS, Done, TaC coating sintering 
Monday, October 17, 2022, 10:03
The coated container was wrapped in 4 Ta foil heatshields. (The 4 shields appear to work well)
Target temperature on OMEGA= 1850-1900 C
Entry  Tuesday, October 25, 2022, 12:25, Darwin Ortiz Rosales, TaC, 44139-15-SK, LP-SIS, Done, TaC coating sintering 
Tuesday, October 25, 2022, 12:18
Container wrapped in 4 Ta foil heatshields
Target temperature on OMEGA= 1850-1900 C
Entry  Friday, October 28, 2022, 07:59, Darwin Ortiz Rosales, TaC, 45220-6, LP-SIS, Done, TaC coating sintering 
Friday, October 28, 2022, 07:58
The coated container was wrapped in four Ta foil heatshields.
Target temperature on OMEGA= 1850-1900 C
Entry  Thursday, November 10, 2022, 07:40, Darwin Ortiz Rosales, TaC, 45220-13, LP-SIS, Done, TaC coating sintering 
Thursday, November 10, 2022, 07:40
The coated container was wrapped in four Ta foil heatshields.
Target temperature on OMEGA= 1850-1900 C
Entry  Friday, November 18, 2022, 15:13, Darwin Ortiz Rosales, TaC, 45220-1, LP-SIS, Done, TaC coating sintering 
Friday, November 18, 2022, 15:08
The coated container was wrapped in four Ta foil heatshields.
Target temperature on OMEGA= 1860-1900 C
Entry  Tuesday, November 22, 2022, 14:59, Darwin Ortiz Rosales, TaC, 45220-12, LP-SIS, Done, TaC coating sintering 
Tuesday, November 22, 2022, 14:58
The coated container was wrapped in four Ta foil heatshields.
Target temperature on OMEGA= 1860-1900 C
Entry  Thursday, March 16, 2023, 14:47, Darwin Ortiz Rosales, TaC, 45220-9, LP-SIS, Done, TaC coating sintering 
Thursday, March 16, 2023, 13:38
The coated container was wrapped in four Ta foil heatshields.
Target temperature on OMEGA= 1860-1900 C
Entry  Thursday, March 30, 2023, 12:45, Aaron Schmidt, Ta, 45220-7, LP-SIS, In progress, Conditioning Ta#65 
Thursday, March 30, 2023, 12:27: 
Ta#65 LP-SIS target description: 
Total Ta foils = 470 [6x20 packs + 350 single discs]
Entry  Sunday, April 16, 2023, 14:08, Darwin Ortiz Rosales, TaC, 45220-14, LP-SIS, Done, TaC coating sintering 
Sunday, April 16, 2023, 14:08
The coated container was wrapped in four Ta foil heatshields.
Target temperature on OMEGA= 1860-1900 C
Entry  Tuesday, April 18, 2023, 06:48, Darwin Ortiz Rosales, TaC, 45220-11, LP-SIS, Done, TaC coating sintering 
Tuesday, April 18, 2023, 06:46
The coated container was wrapped in four Ta foil heatshields.
Target temperature on OMEGA= 1830-1900 C