Wednesday, November 06, 2013, 17:36, John Wong, TaC, Target Boat #2, , In progress, Testing TaC matrix coating
|
The purpose of this experiment is to improve the TaC coating mixed with other metals as additives. The coating solution will be sprayed on Ta metal
(0.015" thick, same thickness as the target container).
The samples will be sintered at ~ 1800C. Once the process is completed, a graphite tube will be inserted into the tube, and then re-heated |
Wednesday, January 15, 2014, 17:45, John Wong, Empty, 39165-9, LP-SIS, In progress, Sintering TaC coating container
|
Wednesday, January 15, 2014, 17:30
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min. |
Friday, January 17, 2014, 09:34, John Wong, Empty, 39165-9, LP-SIS, In progress, Sintering TaC coating container
|
Laura Lambert wrote:
|
Friday, January 17, 2014, 12:52, John Wong, Empty, 39165-9, LP-SIS, In progress, Sintering TaC coating container
|
Laura Lambert wrote:
|
Wednesday, January 22, 2014, 15:13, John Wong, Empty, 40282-4, TARGET BOAT, , Sintering Ta target boat with TaC coating
|
Laura Lambert wrote:
|
Wednesday, January 22, 2014, 18:22, John Wong, Empty, 40282-4, TARGET BOAT, Problems, Sintering Ta target boat with TaC coating (IEVAP2:TBHT2 water signal problem)
|
John Wong wrote:
|
Friday, March 07, 2014, 22:25, John Wong, , 40282-3, TARGET BOAT, Problems, Sintering TaC coated end caps
|
Laura Lambert wrote:
Friday, March 07, 2014, 11:41 |
Monday, March 10, 2014, 11:45, John Wong, , , , Maintenance, Replaced Backing Pump hose
|
Monday, March 10, 2014, 11:44
Rick replaced the backing pump hose from 1.5" to 2.0" for better flow. And the HEPA filter was checked - it looks OK.
|
Monday, March 10, 2014, 11:52, John Wong, , , , Problems resolved, The Chiller is down
|
Monday, March 10, 2014, 11:45
The chiller tripped off on March 7, 2014.
Water is not flowing into the chiller; paddle wheel shows no signal.
Tried turning on the chiller locally; a few seconds |
Friday, March 21, 2014, 16:18, John Wong, TiC, 38817-8, HP-SIS, In progress, Sintering TiC
|
Friday, March 21, 2014, 16:09
Target container is loaded with 360 Discs of TiC.
Target length = 11.7cm. |
Wednesday, March 26, 2014, 18:23, John Wong, TiC, 38817-8, HP-SIS, Done, Sintering TiC#4
|
Laura Lambert wrote:
|
Thursday, March 27, 2014, 18:04, John Wong, , , TARGET BOAT, In progress, Studying WC sintering on Ta surface
|
Thursday, March 27, 2014, 17:38
TEST #1
WC slurry was prepared in non-aqueous environment (see lab book for procedures). The solution was dripped on two Ta plates (3.1cm2) and let |
Thursday, April 24, 2014, 18:13, John Wong, , , TARGET BOAT, Done, Tests: Sintering carbon Mesh coated with WC
|
Thursday, April 24, 2014, 17:25
The purpose of this experiment is to see if the carbon mesh is suitable for coating and sintering with uranium carbide. For this test, the
mesh is coated with WC slurry (previously prepared). |
Monday, June 16, 2014, 17:42, John Wong, Ta, 40282-2, LP-SIS, In progress, Conditioning Ta#43 target
|
Laura Lambert wrote:
Friday, June 13, 2014, 14:53 |
Friday, June 20, 2014, 16:22, John Wong, SiC, 39530-8, HP-FEBIAD, In progress, Conditioning SiC#31 target
|
Laura Lambert wrote:
Friday, June 20, 2014, 11:14 |
Tuesday, June 24, 2014, 23:57, John Wong, SiC, 39530-8, HP-FEBIAD, In progress, Conditioning SiC#31 target
|
Laura Lambert wrote:
|
Wednesday, July 23, 2014, 15:07, John Wong, Empty, 40282-3, LP-SIS, In progress, Sintering TaC coated target container
|
Wednesday, July 23, 2014, 15:07
Target container is coated with TaC. No Ta-heat shields are used.
TGHT will be ramped up to 580A at 0.2A/min. |
Tuesday, July 29, 2014, 11:23, John Wong, , 40282-3, LP-SIS, In progress, Sintering ZrC# 6 target
|
Laura Lambert wrote:
Monday, July 28, 2014, 14:41 |
Tuesday, August 05, 2014, 17:20, John Wong, , , TARGET BOAT, In progress, Sintering TaC coated end caps
|
Laura Lambert wrote:
Tuesday, August 05, 2014, 12:02 |
Wednesday, August 06, 2014, 16:10, John Wong, Ta, 38817-9, HP-SIS, In progress, Conditioning Ta target
|
Wednesday, August 06, 2014, 15:59
Target consists of 400 Ta discs.
Total packed length 4.5cm |
|