104
|
Tuesday, January 21, 2014, 11:33 |
Laura Lambert | Empty | 40282-4 | TARGET BOAT | | Sintering Ta target boat with TaC coating |
|
|
|
105
|
Tuesday, January 21, 2014, 11:56 |
Laura Lambert | Empty | 40282-4 | TARGET BOAT | | Sintering Ta target boat with TaC coating |
|
|
|
106
|
Wednesday, January 22, 2014, 09:49 |
Laura Lambert | Empty | 40282-4 | TARGET BOAT | | Sintering Ta target boat with TaC coating |
|
|
|
107
|
Wednesday, January 22, 2014, 13:46 |
Laura Lambert | Empty | 40282-4 | TARGET BOAT | | Sintering Ta target boat with TaC coating |
|
|
|
108
|
Wednesday, January 22, 2014, 15:13 |
John Wong | Empty | 40282-4 | TARGET BOAT | | Sintering Ta target boat with TaC coating |
|
|
|
109
|
Wednesday, January 22, 2014, 18:22 |
John Wong | Empty | 40282-4 | TARGET BOAT | Problems | Sintering Ta target boat with TaC coating (IEVAP2:TBHT2 water signal problem) |
|
|
|
110
|
Thursday, January 23, 2014, 16:22 |
Laura Lambert | Empty | 40282-4 | TARGET BOAT | Problems resolved | Sintering Ta target boat with TaC coating |
|
|
|
111
|
Friday, January 24, 2014, 14:25 |
Laura Lambert | Empty | 40282-4 | TARGET BOAT | In progress | Sintering Ta target boat with TaC coating |
|
|
|
112
|
Monday, January 27, 2014, 10:59 |
Laura Lambert | Empty | 40282-4 | TARGET BOAT | In progress | Sintering Ta target boat with TaC coating |
|
|
|
113
|
Tuesday, January 28, 2014, 11:57 |
Laura Lambert | Empty | 40282-4 | TARGET BOAT | In progress | Sintering Ta target boat with TaC coating |
|
|
|
114
|
Tuesday, January 28, 2014, 13:09 |
Laura Lambert | Empty | 40282-4 | TARGET BOAT | Done | Sintering Ta target boat with TaC coating |
|
|
|
115
|
Tuesday, January 28, 2014, 15:46 |
Laura Lambert | | 40282-4 | TARGET BOAT | Failed | Sintering TaC coated end caps | Tuesday, January 28, 2014, 15:43
The target containers end-caps were
coated with TaC spray and let dry. |
|
|
118
|
Tuesday, February 18, 2014, 12:19 |
Laura Lambert | Empty | 40282-3 | TARGET BOAT | Done | Sintering Ta target boat with TaC coating | Tuesday, February 18, 2014, 12:12
A new target boat was sprayed with
TaC coating and let dry. |
|
|
119
|
Tuesday, February 25, 2014, 16:10 |
Laura Lambert | | 40282-3 | TARGET BOAT | Done | Sintering TaC coated end caps | Tuesday, February 25, 2014, 16:08
The target containers end-caps |
|
|
121
|
Friday, March 07, 2014, 11:46 |
Laura Lambert | | 40282-3 | TARGET BOAT | In progress | Sintering TaC coated end caps | Friday, March 07, 2014, 11:41
The target container end-caps were
sintered previously, but did not fully complete |
|
|
122
|
Friday, March 07, 2014, 22:25 |
John Wong | | 40282-3 | TARGET BOAT | Problems | Sintering TaC coated end caps |
|
|
|
128
|
Thursday, March 27, 2014, 18:04 |
John Wong | | | TARGET BOAT | In progress | Studying WC sintering on Ta surface | Thursday, March 27, 2014, 17:38
TEST #1
WC slurry was prepared in non-aqueous |
|
|
129
|
Thursday, April 24, 2014, 18:13 |
John Wong | | | TARGET BOAT | Done | Tests: Sintering carbon Mesh coated with WC | Thursday, April 24, 2014, 17:25
The purpose of this experiment is
to see if the carbon mesh is suitable for |
|
|
130
|
Thursday, May 29, 2014, 18:16 |
Cameron Hodgins | | | TARGET BOAT | In progress | Sintering several carbides on tantalum foil backing | Purpose: Sinter one sample of each of TiC,
VC, Cr3C2, ZrC, NbC, Mo2C, TaC, and WC on
5x10 mm tantalum foil to see if the samples |
|
|
132
|
Friday, June 06, 2014, 16:01 |
Cameron Hodgins | | | TARGET BOAT | In progress | Sintering several carbides on tantalum foil backing | Auto-ramp started. Max current = 500 A,
voltage = 11.05 V. Current is being increased
at 2 A/min. In the first 20 minutes, the |
|