Sunday, July 22, 2012, 20:30
The NiO target materials were loaded into the container today.
Total discs = 500, (10 discs/pack)
length (after loaded) = 9.0cm
Target container is wrapped with Ta-heat shields, and will be removed after the sintering process.
One regular end cap is inserted (with Ni-foil inserted as a divider). The caps, however, are very loose (tried 2 caps and still loose). Hopefully the thermo diffusion bonding will seal the cap...
The other end is inserted with a D-cap for out-gassing proposes, and will be replaced with the regular end-cap after the process.
(see attachment#1)
Sunday, July 22, 2012, 20:48
The camber has been pumped down and currently IG1=1.3e-6 Torr.
The HS cooling water was turned on and no leaks were detected.
TGHT and TBHT were stepped up to 50A.
Auto-ramping is initiated at 0.2A/min for TGHT max = 250A, TBHT max = 230A.
Thursday, July 26, 2012, 23:31
TGHT and TBHT have reached to 250A (local @ 242A/2.88V) and 230A, respectively, and have stayed for ~4hrs (see attachment#2)
Currently, IGP1 = 4.9e-7 Torr, IGP2 = 3.5e-7 Torr, CG1B = 13mTorr.
Initiating auto-cool down at 2A/min.
Monday, July 30, 2012, 15:11
The chamber was vented and the target was removed.
There was significant condensation oily fluid coated Cu-heatshield lid and around the ionizer opening.
Overall, the target looks very good. The NiO target material was nicely sintered. No shrinkage or loose particles were observed (see attachment #3).
The endcap, however, was not properly fitted and it just fell off, (see attachment #4).
Both ends of the target are currently opened; the expension tool for the endcap is in order and hopefully this will solve the problem.
The target is being stored in the fumehood
|