Thursday, April 20, 2017, 12:38
3 samples are loaded into the Ta boat and wrapped with heat shield (1 long piece, 3 rounds): 2x of B3-92Mpa pellets and 10% pure PAN pellet as control. See lab book page 32 for more details.
The B3-92Mpa pellets were previously heated to 1550C (TGHT 400A/6.94V), see elog#351
Attempting to heat samples up to 1800C to determine the weight loss and shrinkage.
Est. TGHT 480A.
OK to auto ramp to 400A at 1A/min. Check for coating on the window.
Chamber is currently being pumped down.
Thursday, April 20, 2017, 14:28
Pressure 3.14e-6 Torr. Auto ramp TGHT at 1A/min to reach 400A.
Friday, April 21, 2017, 10:56
TGHT at 400A/6.75V, temp at 1475C (75C/0.19V lower).
Tapping up TGHT
Friday, April 21, 2017, 12:32
TGHT ramped up to 530A/9.85V, temp at 1800C.
Friday, April 21, 2017, 15:38
TGHT dropped slightly, no coating on windows.
Checked with Mikron, agreed with the dropped temp.
Tapped up TGHt to 545A/10.1V to reach 1800C. Will keep at that temp for several days.
Wednesday, April 26, 2017, 17:06
Samples have been heated at 1800C (-25C) for 7 days now (see attachment for archiver).
Cooling down TGHT at 1A/min.
|