Monday, May 06, 2013, 14:29
UO2/C green was prepared on May 2, 2013 and let dry over the weekend.
UO2 powder used = 50.36g (Inventory R-00835A UO2 + bottle = 896.30)
Graphite powder used = 10g
The green was rolled up and wrapped in a piece of graphite sheet.
The Ta-target boat was wrapped with 3-Ta heat shields and installed in the Evap#1
The chamber is currently being down down.
The target will be ramped up to 520A at the rate of 0.1A/min.
Vacuum limit stop at 5.0e-5 Torr, backing off at 6.0e-5 Torr.
Tuesday, May 07, 2013, 11:12
Currently, IG @ 5.6e-6 Torr; BP @ 25mTorr. Vacuum spikes intermittently...
Stepping up TGHT to 50A. After about 15 min, vacuum climbed up to 5.5e-5 Torr.
Lowered TGHT to 25A, and continue heating at that current...
Tuesday, May 07, 2013, 12:18
Vacuum is coming down to 2.6e-5 Torr.
Auto-heating initiated...
Friday, May 24, 2013, 14:19
The carbonization process has come the end.
TGHT has reached to 520A for ~14hrs.
IG1 @ 6.34e-6 Torr, BP @ 25mTorr.
Autocooling is initiated; ramping rate @ 1A/min.
The chamber will be remained under vacuum, and will be vented in Ar next week.
Monday, May 27, 2013, 14:11
The chamber was vented with Ar.
UC2 was transfered to the Ar glovebox.
Evap#1 is off.
Wednesday, May 29, 2013, 17:14
See attachment#1 for TGHT vs IG1 data retrieval.
|