Thursday, September 29, 2011, 10:54
UO2/C mixture was made on Tuesday Sept 27, casted on a piece of glass and let dried in the fume hood for ~2days.
Dried UO2/C mass = 61.72g
Target material is wrapped /w graphite sheet and put on a new heatboat coated/sintered /w TaC.
Heat boat is wrapped with 3-Ta heat shields.
Evaporator chamber is currently being pumped down.
Friday, September 30, 2011, 10:01
Evaporator has been pumped down over night, IG currently @ 2.92e-6 Torr, BP @ 27mT.
TGHT will be stepped up to 40A and allow the pressure to slowly increase.
Friday, September 30, 2011, 10:30
TGHT is holding at 40A/0.139V (local @ 37A), and pressure is slowly increasing, expect pressure to stabilize at ~4.5e-5 Torr before being auto-heating.
See attachment#1: TGHT_40A.
Friday, September 30, 2011, 13:39
TGHT has been at 40A for more than 3 hrs. Pressure went as high as 6.9e-5 Torr and it's now coming down. (See attachment#2: TGHT@40A_3hrs)
Auto-heating is initiating. TGHT rate @ 0.1A/min to reach to max current of 525A. (see attachment#3: parameter.jpg)
Sunday, October 09, 2011, 10:44
Target heater reached to 520A and held for a few hours.
Evaporator was cooled down last night and TGHT is now at 0A.
(For the overall process, see Attachment#4: UCx#3_batch1.jpg)
IG1 @ 5.7e-7 Torr. Chamber will be vented with Ar on Tuesday.
TGHT is off and water valve is shut.
Tuesday, October 11, 2011, 13:10
Evaporator glovebox was purged with Ar prior to venting the chamber with Ar.
Layers of burnout marks were coated all around the inside of the evaporator (see attachment#5. Evpr_afterprocess.jpg),
Before cleaning, the evaporator chamber had ~200,000 cpm.
The heating boat containing UCx was removed from the evaporator and stored in the "orange" case, then transferred to the Ar-glove box.
Weight of UCx flasks: 47.15g (See attachment#6: UCx#3_batch1_mass.jpg)
The evaporator was thoroughly cleaned; the burnout marks were removed, and it will be used for UCx#3:batch#2 - UO2/C process.
|