Wednesday, July 11, 2018, 17:41
Cast prepared by Marla (see note in Hotlab)
Target boat contained about 50g UO2 powder.
TGHT will be ramped up to 520A.
Vacuum limit stop at 3.0 e-4 Torr, backing off at 6.0e-4 Torr.
Chamber is currently being pumped down
Thursday, July 12, 2018, 10:45
Pressure at 8.9e-7 Torr.
Initiate auto ramping TGHT at 0.1A/min to reach 580A (will monitor vacuum to ensure complete carbonization)
Wednesday, July 18, 2018, 10:23
TGTH at 369A/3.7V, carbonization in progress.
Pressure limited was set to 5.0e-5 Torr; change limit to 6e-4 Torr (as indicated above)
Increase ramping rate to 0.2A/min.
Thursday, July 19, 2018, 12:12
Completion of the U-carbonization has been reached.
Cooling down TGHT at 2A/min
Chamber will be vented in Ar and materials will be transferred to Ar glovebox
|